Also check your solder for metallic impurities. Some favour the formation
of icicles.
Bev Christian
Nortel Networks
> -----Original Message-----
> From: Feng Yi,BISC PD IE(BJ) [SMTP:[log in to unmask]]
> Sent: Wednesday, May 05, 1999 4:38 AM
> To: [log in to unmask]
> Subject: Re: [TN] Icicle formation on wave soldering
>
> Dear Sunil,
> the same problem has been found in our company, and we solved it though
> below mentioned methods.
>
> 1) increase pre-heat tempreture to 160¡æ
> 2)increase the spraying flux
> 3)only use single wave solder, not double wave solder
>
>
> Best Regards
>
>
> Qu Zenglong
>
> Industrial Engineering Department
> Production Division
> BISC, China
> Tel: 0086-10-64346323
> Fax:0086-10-64367731
> e-mail: [log in to unmask]
>
> ----------
> From: Sunil Gupta[SMTP:[log in to unmask]]
> Reply To: TechNet E-Mail Forum.;[log in to unmask]
> Sent: Wednesday, May 05, 1999 11:49 AM
> To: [log in to unmask]
> Subject: [TN] Icicle formation on wave soldering
>
> While wave soldering the mixed technology boards I am facing the
> problem of
> icicles being formed on the solder side. The icicles are only on SMDs
> (capacitors and resistors, there are no other SMDs) while not observed on
>
> lead thru components. The machine parameters are:
> Bath temperature: 245 deg C
> Conveyor speed: 1m per minute
> Fluxing thru foam fluxer
> PCB temperature before soldering: 100 deg C
> Preheat zone length: 1.5 m
>
> The problem got solved by heating the boards at 60 deg C and than
> passing
> them thru the fluxing and soldering.
>
> I want to eliminate the Icicle problem and also remove the
> requirement of
> baking.
> Can you give me ideas.
>
> regards
>
> Sunil Gupta
> Manager Process Engineering
> Tata Telecom Ltd.
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site ( <http://www.ipc.org>) "On-Line Services"
> section for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or
> 847-509-9700 ext.312
> ################################################################
>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|