Stephen,
Have you attached thermocouples around the QFP to verify that the QFP is:
A) Reaching Liquidous?
B) Is at Liquidous for a long enough period of time?
I have had grainy solder joints and found that I was not at liquidous for a
long enough period of time for complete reflow of all of the solder joints.
It was on a very dense assembly and the problem was more in the center of
the assembly.
Just curious.
I have used aluminum fixtures for assembly processes and have never had an
issue with contamination.
Good Luck,
Kathy Palumbo
> -----Original Message-----
> From: Stephen Bonaccorsi [SMTP:[log in to unmask]]
> Sent: Thursday, April 01, 1999 3:34 AM
> To: [log in to unmask]
> Subject: [TN] GRAINY JOINTS
>
> Hello Everybody
>
> I am currently reflowing with a convection oven (No Nitrogen). A board
> that has perfect solder joints apart from grainy solder joints on one
> particular component (QFP). Other components on the board resistors/caps
> and components of similar size are fine.
> Therefore I don't think there is a problem with the oven profile.
>
> This component does go through an extra process before hand.
> Initially the component is supplied with no pins (Very long story,
> don't ask!)
> These are attached to the body of the component using an aluminum
> jig/fixture to hold them in place. The legs are supplied
> pre-soldered.
> RMA flux is then applied (liberally) to the area to be soldered.
> The jigs with the components are then placed through a vapour phase oven
> for soldering .
>
> Is it possible that the legs are being contaminated by Aluminum or its
> oxide from the jig/fixture, if the flux is reacting the Aluminum.
>
> Would aluminum contamination give grainy joints?
> What else can cause grainy joints?
>
> Thanks for any help
>
> Stephen Bonaccorsi
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
> section for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or
> 847-509-9700 ext.312
> ################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|