residue left from active rosin flux will cause corrosion. Normally, form
CuCl2 (green corrosion product) after T/H/B test. The connector location is
difficult to clean if you don't have the proper clearance (standoffs) from
the PWB.
good luck.
jk
At 05:25 PM 4/14/99 MDT, you wrote:
>Has anyone heard of rosin based fluxes causing corrosion?
>
>It is on a connector with solder cup connections and the flux used is
>a RA flux. The pins and the solder is showing signs of corrosion.
>Could this be caused or accelerated by the flux?
>
>Any help is appreciated.
>
>Ryan
>
>-----------------------
>Ryan Chase
>Manufacturing Engineer
>GE Harris
>403-214-4502
>Fax 403-287-3107
>[log in to unmask]
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
>To subscribe: SUBSCRIBE TechNet <your full name>
>To unsubscribe: SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
>################################################################
>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|