Hi Chris
Here are some of the answers as I see them:
We thermally stress circuit boards at 550o F (288o C
) for ten seconds, referencing test method IPC-TM-650, Number 2.6.8.,
revision
C, date 8/97, sections 5.4 - 5.6.
But how often should we replace the solder ?
Is there a time constraint or quantity constraint that dictates when
to replace the solder with new material ?
Since you are using the solder for thermal stress and not solderability,
there are
very few constraints on the solder in the pot since it is a heat source and
it's
composition is not critical to the test.
If you were also using the pot for solderability testing, you would follow
the
recommendations found in J-STD-001.
In addition, is there any information concerning the procedure for
replacing the solder in the pot ?
Is there a percentage of copper that must be added to the 63/37 tin/lead
solder ? Or some other preparation needed for proper solder flow.
As for a complete replacement the solder should be molten and we just
pour it out into another container - very carefully.
You could also cool the bath and skim off material that solidifys first since
it will contain contaminates - such as copper and then add additional fresh
solder.
The solder should flow very well at 63/37, if the samples are properly fluxed
prior to floating.
Hope this helps. Let me know if you need further clarification.
Susan Mansilla
Robisan Lab
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|