I created several R/F designs using a combination of CLTE and GETEK last year. As Ron said,
the stuff be managed well in well managed pre lamination, lamination, and post lamination
phases. Delamination can be a serious issue, but is minimized by those having been down the
road. Another issue is cure. If not properly cured, you can take a pen knife and lightly pick
away at the crumbling surface and deeper as the powdery substance comes apart. This condition
usually is found in areas on/in the board exibiting "blisters" or really serious
delamination.
Not advertising, but the two shops successfully completing both test panels and production
boards were Multek and Praegetzer. I only tried a couple of other local Bay Area shops and
they didn't make the cut.
As Ron said, the "resin" system, for lack of better terminology, is made PTFE, and a ceramic
"frit" that, when coated/treated to the 106 glass style has a tendency to behave in a
difficult way. Arlon and Rogers, who developed the "resin" system, talk about the mixture as
chunky peanut butter being spread on a piece of glass fabric with hopes of making it stick.
Not matter the difficulties, it certainly is attractive from a Dk standpoint. 2.94 is getting
closer to air and, when successfully laminated, offers excellent dimensional properties.
Earl Moon
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|