Steve,
The current density on your stress tabs is directly proportional to the
total current density that is applied to the Hull cell. So, if you ran
your Hull cell at 3.75 amps, the current density on the third tab would be
27 ASD. The problem is that the current density on your first tab would
reach 45 ASD! Depending on the degree of agitation you can provide, the
temperature of the electrolyte and the nickel concentration, your first and
second tabs are likely to "burn", which might alter their internal stress
value. Another option might be to set the current at 2.25 amps, which will
translate into 27 ASD on your first tab and disregard the higher current
density region.
Eric Yakobson
Alpha PC Fab
Schram Steve <[log in to unmask]> on 01/26/99 06:18:57 AM
To: [log in to unmask]
cc: (bcc: Eric Yakobson/AlphaPCFabUS/Cookson)
Subject: [TN] Stress Testing
This is the first time I have used this e-mail system. We are not plating
PCB's, we make compact disc, specifically the mold plate used to mold
compact disc. We are not electroplating, we are electroforming, the metal
we are plating on is passivated so there is no bonding of the two metals.
The electroformed piece is completely seperate from its parent when
completed. The mold plate or stamper as we call it has all the music
physically embedded on its surface, as microscopic metal forms (125
nanometers tall x 500 nanometers wide and .5 - 3 micrometers long). The
nickel plates are 149mm in diameter and are plated at a max current of 48
amps to a thickness of 300 micrometers. The current density runs about
27-28 amps/square decimeter.
The test we are performing with the hull cell uses stress tabs, a special
panel with 5 copper foils which only plate on their front sides. The tab
closest to the anode tests the highest current density the tab farthest
away
tests the lowest current density. If set up properly the first and second
tabs (the closest) should curl towards the anode due to tensile stress the
third tab should remain strait and the fourth and fifth should be curled
away from the anode due to compressive stress.
The chart sent with the stress tabs reads as follows:
Amps #1ASD #2ASD #3ASD #4ASD #5ASD
1.0 12 9.6 7.2 4.8 2.4
0.8 7 5.6 4.2 2.8 1.4
0.6 3.5 2.8 2.1 1.4 0.7
0.4 2 1.6 1.2 0.8 0.4
0.2 0.4 .32 .24 .16 .08
As you can see the 1.0 amp is the highest current for the chart and tests a
current density of 7.2ASD on the third tab. My question is how do I
interpolate this chart to test 27ASD on the third tab.
Thanks for your reply, any help is appreciated,
Steve Schram
CD Mastering Manager
Universal Studios, Universal Music and Video Dist.
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|