Hi Steve - I don't know if you have this option available but if the cause
of the solder wicking is due to uneven heating of the pins in the pin
header you might try a vapor phase soldering operation. We have placed the
daisy chained solder donut preforms on similar pin headers, sprayed on flux
, and into the vapor phase equipment they go. We haven't had any problems
other than the occasional "run solder down the pin" issue to poor preform
placement. The condensation heating of the vapor phase operation produced
uniform heating needed to prevent having inconsistent solder joints. Good
Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Stephen R. Gregory" <[log in to unmask]> on 01/12/99 11:59:13 AM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
to [log in to unmask]
To: [log in to unmask]
cc:
Subject: [TN] Assy:Through-hole Solder Preforms...
Good Day Ya'll!
We just got a new customer here last week and built two 10-board proto
kits for them. Those boards are a type of power supply, and we're going to
be
doing another board that they call a 4-port RS-232 + 48 digital I/O PC/104
Module. All 3 assemblies are roughly 3.5" square and are mixed technology.
There's another thing common between all three assemblies besides
their
size, what they call dual-mount headers. Each board has two of these, one
is a
64-pin (2X32 pins), and the other is a 40-pin (2X20 pins). These are
basically
real long gold plated headers with plastic female type receptacles at one
end.
They're installed with the header pins going THROUGH the board and
soldered.
The header pins stick out the backside of the board 10mm, and you have your
female sockets on the topside, so now what you have is a stackable type of
board connection system.
Cool connection system, BUT, there's a big problem with soldering these
dad-
blamed things! You can't wave solder them because: 1.) They're gold plated,
no
solder on the contact area (solder fillet must stay below .100" as measured
up
the pin from the surface of the PCB). 2.) Even if the gold plating wasn't
an
issue, they stick out 10mm on the bottom...you'd need a wave that shoots up
and looks like "Old Faithful" to reach the bottom of the board!
"So hand solder em' ya big weenie!" some of you may be muttering under your
breath now. Well there's a problem there too. The way these two connectors
are
laid-out on the boards couldn't be any worse, they're parallel right next
to
each other, spaced .100" apart. We've got 4-rows of 10mm long gold plated
pins, .100" apart, that we've got to solder and not get any solder on the
gold
plating...just peachy huh?
My senior rework lady Trang, got us through the two proto kits of
20-boards.
She somehow was able to thread her soldering iron down thru the pins and
solder the connectors in without so much as a pimple of solder on the pins
(She simply amazes me sometimes! Goes to show what clean livin' and no
caffeine can do for ya!) But we simply can't do that in production, it'll
take
forever, and I don't wanna burn Trang out, she's the only one steady enough
to
do it.
So I called around to get quotes on some preforms. I've seen daisy-chained
donut preforms that you can use for headers and what have you that has the
same kind of footprint. I've used preforms before, but the kind for edge
clips
for little SIP modules, not for PTH. So I called Indium, AlphaMetals, Bow
Solders, and Kester...they all make preforms. Everybody has quoted me, but
Kester told me that they think I may still may have a problem. They said
that
from their experience, I'm going to have difficulty obtaining consistent
solder joints using preforms. They said that unless I can ensure very
consistent heating between all the pins, that I'll probably wind-up with
some
joints being insufficient because the solder will tend to wick to the
hottest
pin. I was planning on using a heat gun to provide the heat, and maybe even
going so far as to make a nozzle that will enclose all the pins. But I
can't
put it in a reflow oven unless I want to hand solder eight 10-pin SIP
RPACKS,
and a 2-pin metal canned crystal afterwards...I still need to look and see
if
the plastic on the headers can take the heat anyway.
So after reading this journal, my question is (boy, I sure take the scenic
route sometimes don't I?); have any of you had any experience with the kind
of
preforms I'm thinking of using? Is what Kester saying true?
'Preciate any info at all!!
-Steve Gregory-
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|