Kelly,
There are additional factors that will influence throwing power in a plated
through hole. Three factors to keep in mind are (1) concentration
polarization (2) polarization from charge transfer and (3) resistance opr
voltage drop through the hole. The surface does not have the voltage drop.
Therefore, unless you can overcome resistance or increase the polarization
due to charge transfer, you are doomed to plate more copper on the surface
than in the hole.
Best regards,
Michael Carano
-----Original Mesage-----
From: Eric Yakobson <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Date: Tuesday, November 10, 1998 11:00 AM
Subject: Re: [TN] Copper plating & Copper thickness
>Kelly,
>
>The greater is the difference in the cathode polarization (on high/low
>current density points of the cathode) -- the more uniform is the current
>distribution.
>
>It is really difficult to properly explain this statement without going
>into the details and definitions of primary/secondary current distribution,
>overpotential and polarization, which without any doubt would bore most
>TechNetters to death.
>
>To put it simplistically, high polarization on high current density points
>means that actual current density on them is lower then it otherwise would
>have been if this polarization did not exist.
>
>If you would like to discuss this subject any further, please contact me
>off line.
>
>Eric Yakobson
>
>
>
>
>Kelly Kovalovsky <[log in to unmask]> on 11/09/98 07:21:58 AM
>
>To: [log in to unmask]
>cc: (bcc: Eric Yakobson/AlphaPCFabUS/Cookson)
>Subject: Re: [TN] Copper plating & Copper thickness
>
>
>
>
>Your note is interesting and educational for me and I appreciate your time
>and
>effort in providing this detail.
>
>I have a follow on question that maybe you can help me with. If I may
>restate
>your second paragraph I would say:
>
>At high average current density the cathode polarization difference between
>low
>and high current points is more uniform (To me, less difference means more
>uniform) and therefore the current distribution is less uniform.
>
>I may not understand cathode polarization correctly, but I assume from your
>statement that there is an inverse relationship between the uniformity of
>cathode polarization and the uniformity of current distribution. Please
>confirm.
>
>Kelly Kovalovsky
>
>
>
>
>[log in to unmask] on 10/31/98 08:41:39 PM
>Please respond to [log in to unmask]
>To: [log in to unmask]
>cc:
>Subject: Re: [TN] Copper plating & Copper thickness
>
>
>Michael,
>
>With all due respect, I'm afraid I have to disagree with your explanation.
>While it is true that cathode current efficiency for a typical acid copper
>electrolyte is close to 100%, this is exactly the reason why it does not
>have any effect on current distribution. The key to the explanation of
>this phenomenon is cathode polarization (sorry for the electrochemical
>terminology, but it would be rather difficult to explain this without using
>it).
>
>At low average current density the difference between cathode polarization
>on lower/higher current density points of the cathode in most electrolytes
>(including acid copper) is normally much greater than at high average
>current density. Therefore, the current distribution is more uniform at
>low average current density.
>
>In most alkaline electrolytes, where current efficiency is much lower than
>100% (the rest of the current is consumed for hydrogen gas evolution), it
>does affect the current distribution favorably. Since at higher densities
>more current is consumed for hydrogen evolution, the metal distribution
>generally is more uniform then in acid solutions.
>
>Low current density will result in higher throwing power in both systems.
>One of the few practical exceptions to this rule (low current density/high
>throwing power) is hex-chromium electrolyte, in which current efficiency is
>directly proportional to current density.
>
>As to the minimum copper thickness, historically (by trial & error I guess)
>it was determined that 1 mil (25 micron) of copper is a minimum thickness
>that will reliably withstand multiple solder floats. From my practical
>experience, 0.5 mil cracks much more readily, which is understandable,
>considering the fact that copper tensile strength is proportional to the
>thickness of the deposit.
>
>Best regards.
>
>Eric Yakobson
>Alpha PC Fab
>
>
>
>
>
>
>mcarano <[log in to unmask]> on 10/31/98 07:30:36 AM
>
>To: [log in to unmask]
>cc: (bcc: Eric Yakobson/AlphaPCFabUS/Cookson)
>Subject: Re: [TN] Copper plating & Copper thickness
>
>
>
>
>Dear Francis,
>
>The best explanation for any type of electroplating in an acid medium has
>to
>do with plating efficiency. Generally, acid plating process like the acid
>copper, acid tin etc are close to 100% efficient. In other words, the
>plating favors the high current dednsity areas of a pwb(the surface as
>opposed to the hole) By lowering the cathode current density, you now tend
>to favor the low current areas somewhat, and thus improve throwing power.
>This works just the opposite with alkaline based plating solutions.
>
>With respect to high frequency and plating unformity, I am not sure.
>Generally, the more thickness inside the hole, the better the hole wall
>plating is able to stand up to thermal excursions.
>
>Hope this helps.
>
>-----Original Message-----
>From: Francis Lai <[log in to unmask]>
>To: [log in to unmask] <[log in to unmask]>
>Date: Saturday, October 31, 1998 9:30 AM
>Subject: [TN] Copper plating & Copper thickness
>
>
>>Dear Sir :
>>
>>I work inn a high frequency PCB manufacturing company and I have the
>>
>>following questionns :
>>
>>1/ Why is it for copper plating (acid copper plating) the lower the
>> current, the more the throwing power ? If I start to plate copper
>> on the PTH walls with high current density after PTH, what will
>> happen ?
>>
>>2/ Our customer always specify to have a certainn thickness innside the
>> PTH walls for copper. Why is that so for high frequency PCB ?
>> What happen if copper thickness is thinner than the specified
>> thickness at high frequencies ?
>>
>>Thanks for your help !!!!!!!
>>
>>my e-mail : [log in to unmask](this is only text base, pls do not
>send
>> graphics)
>>
>>Thamks again!!!!!!!
>>
>>Francis
>>
>>################################################################
>>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>>################################################################
>>To subscribe/unsubscribe, send a message to [log in to unmask] with
>following
>text in the body:
>>To subscribe: SUBSCRIBE TechNet <your full name>
>>To unsubscribe: SIGNOFF TechNet
>>################################################################
>>Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
>section
>for additional information.
>>For technical support contact Hugo Scaramuzza at [log in to unmask] or
>847-509-9700 ext.312
>>################################################################
>>
>>
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
>text in the body:
>To subscribe: SUBSCRIBE TechNet <your full name>
>To unsubscribe: SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
>for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
>847-509-9700 ext.312
>################################################################
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
>text in the body:
>To subscribe: SUBSCRIBE TechNet <your full name>
>To unsubscribe: SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
>for
>additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
>847-509-9700
>ext.312
>################################################################
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
>To subscribe: SUBSCRIBE TechNet <your full name>
>To unsubscribe: SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
>################################################################
>
>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|