TECHNET Archives

November 1998

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain
Sender:
Subject:
From:
Bill Davis <[log in to unmask]>
Date:
Mon, 30 Nov 1998 12:08:11 -0800
MIME-Version:
1.0
X-To:
"Kady, Kevin P" <[log in to unmask]>
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Bill Davis <[log in to unmask]>
Parts/Attachments:
text/plain (94 lines)
Kevin:
Below are Wolfgang's & Jim's info... Contact Jim for his chart...

Regards,
Bill Davis, Ph.D.
Diamond Multimedia Systems
Senior Scientist
Tel. 408.325.7868
Cell. 408.888.5650
e-mail: [log in to unmask]

======================================================================
x/y = 10-12 *10^(-6)/K  (Klein-Wassik: softsolder in the elektronics, or
how
it may be called in a non-german edition)
Kett-richtung (bended fibers) 12* 10^(-6)/K  (privat comunication by an
sellman)
Schuss-Richtung (straight fibers) 14-15 * 10^(-6)/K  (privat
comunication by
an sellman)
z = 50-70  10^(-6)/K  (privat comunication by an sellman)

Hope it helps

Wolfgang Nuechter
=======================================================================
I have a comprehensive chart which I can fax you, if you want to provide
the
phone #.
Generally, Z-axis is 60 to 80 ppm (or microinches/inch/C), X is 17-20
ppm, and
Y is 15 to 18 ppm.  Lots of variables however:
a.  These values are for a temp ramp up to the Tg, which is 135C
typically for
FR4.
b.  Remember that FR4 today can be a material with a Tg as high as 180C.
Higher Tg FR4's tend to exhibit a slightly lower Z-expansion below the
Tg than
135C types.
c.  Z-axis is particularly affected by resin:glass ratio.  Higher Resin
content means greater expansion, which has to be considered in high
layer
count designs.
d.  Above the Tg,  the X and Y movements get squirrelly because the
softened
resin allows the glass fabric to pull back against the expanding matrix,
resulting in much lower values.
jimpaulus

>
>
>


-----Original Message-----
From: Kady, Kevin P [mailto:[log in to unmask]]
Sent: Monday, November 30, 1998 9:37 AM
To: [log in to unmask]
Subject: [TN] FR4 properties


Hello,
I am interested in the material properties of FR4, particularly, the
coefficient of thermal expansion.  Can anyone help?
Thank you,
Kevin Kady

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV
1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with
following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
################################################################

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################


ATOM RSS1 RSS2