Hi Glenn,
A bi-level gold approach, i.e., 10 to 20 u" over everything, and 70 U'
min. at the wire bond sites, is the simplest way to go, if you can
tolerate the 10 to 20 u" of gold in your solder process. At least,
this approach requires the least amount of imaging or masking steps
and generally provides better yields at the board fab level. It most
often is the least expensive approach as well, unless there very large
features that are consuming gold.
Hope this helps.
If you want to discuss this further, you can contact me off-line.
Andy Slade
HADCO Tech Center East
978-556-6310
______________________________ Reply Separator _________________________________
Subject: [TN] Fab: Multiple surface finishes
Author: glenn pelkey <[log in to unmask]> at SMTPLink-Hadco
Date: 09/30/98 10:31 AM
Hello all,
I'm looking for information on how to build a board with both soft
gold and solder as outer layer surface finishes. We want to make sure
it is manufacturable before designing it. The only thing I have now are
examples with edge connectors. The gold and solder would be at select
locations throughout the board.
In case you're wondering why, I'll tell you. We want to increase
the gold thickness to greater than 70 microinches for wire bonding.
But, this product also has screened solder for SMT. Since sceening
limits the amount of solder, gold embrittlement becomes an issue. I
calculated 3.7% of gold by weight at 70 microinches. I know opinions
vary here, but I think everyone can agree that this is at least a
concern.
What do you think? How hard is this to do? Contamination,
increased cost, other reliabilty or quality issues to trade off?
Thanks for all your help.
Glenn Pelkey
Maxtek Components Corp.
[log in to unmask]
[log in to unmask]
______________________________________________________
Get Your Private, Free Email at http://www.hotmail.com
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text
in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for
additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700
ext.312
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|