In-Reply-To:
Content-Type:
TEXT/PLAIN; charset=US-ASCII
MIME-Version:
1.0
Parts/Attachments:
TEXT/PLAIN (66 lines)
Mr Engelmaier,

Are you sure about some of the statements made, with regards to Ag and gold
being similarly solderable, and that the nickel is a means of gaining a
solderable surface?

Nickel underplate is simply a diffusion barrier for copper, upon which the
gold is plated to prevent the nickel from tarnishing. A copper surface (not
sure about brass) is very solderable, hence the development of OSPs, and
the like, however, gold cannot be used as a solderability preservative on
top of the copper because the copper will diffuse through the porous gold,
hence, nickel is first plated, followed by a typical, 8 microinches gold
layer. Too thick a gold deposit will lead to solderability issues with the
Au-Sn intermetallic, hence the ratio of solder thickness to gold thickness
must be controlled closely, to achieve a good bond. Thermosonic wire
bonding has different parameters.

LK

On Thu, 1 Oct 1998, Werner Engelmaier wrote:

> Hi Neil,
> Are you sure you have de-wetting? You may never have had any wetting in the
> first place or you may have too much brittle and weak Au-Sn and/or Ag-Sn
> intermetallic compounds (IMCs) near the interface, which with  upwards of 2
> microns of Ag or Au, and particularly with 2 microns each of Ag AND Au, is
> likely. You can tell the difference by analyzing the lead surface. If there is
> little or no Sn present, you never had wetting, if you have Sn and Ag/Au
> present it is the IMCs.
> The Ag does not reduce solderability, it is similar to Au in this respect.
> With this much Au/Ag underplating with nickel will NOT help. The Ni-underplate
> only helps if the brass is not solderable by itself.
>
> Werner Engelmaier
> Engelmaier Associates, L.C.
> Electronic Packaging, Interconnection and Reliability Consulting
> 7 Jasmine Run
> Ormond Beach, FL  32174  USA
> Phone: 904-437-8747, Fax: 904-437-8737
> E-mail: [log in to unmask]
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
> To subscribe:   SUBSCRIBE TechNet <your full name>
> To unsubscribe:   SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
> ################################################################
>
>

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################


ATOM RSS1 RSS2