As I am unsure how to correctly address you, I hope you will not mind me
referring to you as Lum.
I think that your problem is probably related to coating material that is
under the power module. Despite this being mounted flush to the board, the
coating material generally exhibits a low surface energy and/or high level
of capillarity.
Because the power module probably has a high thermal efficiency, I would
assume that there is uncured material underneath. What you could be seeing
is residual solvent gasses that have pushed through the coating material.
It could be trapped air, but I doubt it.
Solution: Try an extended heat cure on the coating for 24 hours at 80 deg C,
but leave sufficient time for the coating to "rest" before putting in the
oven - yeh! - Its a bit like baking bread!
If you could let me know what the coating material is, I may be able to give
you more info.
Regards, Graham Naisbitt
[log in to unmask]
Concoat Ltd Phone: +44 1276 691100
Alasan House Fax: +44 1276 691227
Albany Park
CAMBERLEY
GU15 2PL UK
Any opinions expressed are those of this employer.
-----Original Message-----
From: Lum Wee Mei <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Date: 01 September 1998 03:29
Subject: [TN] Bubbles from conformally coated board
>The test engineer came back to us to complain that bubbles are found
>along the edge of the power modules after going through the temperature
>cycling tests. This problems are found on both coated boards. The power
>modules are mounted completely flushed onto the board and subject to
>conformal coating using the diping method. The coated board undergo QC
>to ensure all components are completely coated, inlcuding the edges
>around the modules.
>
>What could be the problem?
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
>To subscribe: SUBSCRIBE TechNet <your full name>
>To unsubscribe: SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
>################################################################
>
>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|