Try Winslow Automation, they sell preforms for reballing. www.solderquik.com
(408) 526-1213.
Also check the recent TechNet archives. Lots of company names came up when
I searched.
The process of reballing a BGA using preforms is quite simple:
1. Bake the parts out before you begin. Some of the BGAs are very
sensitive to moisture.
2. Remove the old solder with solder wick and a good (low temperature)
soldering iron. EasyBraid makes a fancy solder wick which covers the entire
BGA. You will need a custom tip for your iron.
3. Clean the part thoroughly then spread on a paste flux with a small brush
then drop the preform into a fixture together with the fluxed BGA.
4. After reflow you simply moisten the paper and peel it away. Be sure to
clean the BGA thoroughly as most ball attach fluxes are organic acid type.
I hope this helps, [log in to unmask]
-----Original Message-----
From: XO Tronic Ltd. <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Date: Monday, July 27, 1998 4:18 AM
Subject: [TN] BGA reballing equipment
> We are looking for buying an equipment for BGA reballing. Can anyone let
me know where I can get it from. Also grateful if someone can let me know
about reballing process. We are contract manufacturer of SMT/Th.hole boards.
>
>Thanks in advance.
>
>Ashok Tiwari
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|