Auger would work well for this type of system. There are no overlap peaks
and light elements are seen with excellent results. Depth profiling should
determine if the P is on the surface or a sub surface barrier layer.
At 01:17 AM 7/20/98 -0400, you wrote:
> Below is a question about solderability of electroless nickel.
>
>
>______________________________ Forward Header
>__________________________________
>Subject: Analysis
>Author: Edwin Louis at cmd-cs4-cc-p
>Date: 7/10/98 3:52 AM
>
>
> Dan, here is the message I was trying to send to Peter.
>
>
>______________________________ Forward Header
>__________________________________
>Subject: Analysis
>Author: Edwin Louis at cmd-cs4-cc-p
>Date: 7/10/98 3:03 AM
>
>
> Peter we have some electroless nickel on aluminum in which some
>times
> you can solder to it with Sn63 and RMA flux and other times you
> cannot. Some people have suggested that there are various plating
> types per various specs. that incorporate higher or lower amounts
>of
> phosphorus. The high phosphorus containing plating presumedly do
>not
> solder as well as the lower content plating. Another difference I
> understand is that sometimes there are impurities of organics that
> interfere with the soldering or perhaps heavy metal impurities that
>
> interfere with solderability. We would like to analyze and compare
>the
> two types of plating for these impurities. What do you suggest and
>for
> how many dollars?
> It appears after conversation with Dan Sostak that perhaps Auger
> would be best because phosphorus probably migrates to the surface
>as
> do organics. Because of the surface soldering process the culprits
>are
> probably on the surface. As far as trace included organics are co
> ncerned, will microscopic FTIR fit the bill? I would appreciate
>some
> guidance from you on this matter.
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
>To subscribe: SUBSCRIBE TechNet <your full name>
>To unsubscribe: SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
>################################################################
>
>
Tamara E. Bloomer
Assistant Scientist
Ames Laboratory
137 Wilhelm Hall
Ames, IA 50011
(515) 294-2564
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|