Rudy -
I'm surprised to hear that you think 4 microns of nickel is thin.
This is 0.16 mils, & many people specify down to 0.10 mils. You're
suggesting putting on almost « mil of nickel (2-3X of 4 microns)?
Matt Byrne
Hadco-Owego
______________________________ Reply Separator _________________________________
Subject: Re: [TN] Au/Ni/Cu PROBLEM
Author: "TechNet E-Mail Forum." <[log in to unmask]> [log in to unmask] at
INTERNET-OWEGO
Date: 7/5/98 10:23 AM
In a message dated 98-07-05 03:46:42 EDT, you write:
<<
I am a PCB fabricator in the UK and when we started using the electroless
Nickel and Immersion Gold process we noticed a curious phenomenon. If the
panels are immersed in DI water or mains water after processing, then
exposed to air for a minute or two before drying, the gold has reddish brown
stains in random areas. Although this did not seem to affect solderability
to any noticeable extent, it was not cosmetically attractive.
I would like to have an explanation for this mechanism. The immersion gold
is 0.15 microns max (6 millionths of an inch) over 4 microns (0.00016") of
electroless nickel. As this occurs with DI or mains water, contamination of
the water does not seem to be a factor, but simply exposure to air at room
temperature when the surface is wet. >>
Paul:
Given the thiness of the EN (and Au), I would bet the problem is likely one of
porosity, and having some exposed Copper here and there. And porosity driven
by our industry's great nemisis, galvanic corrosion, would give you exactly
what you are seeing.
Further, I would bet that thicker EN ( 2-3X) would stop the problem.
Rudy Sedlak
RD Chemical Company
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text
n the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for
ditional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700
t.312
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|