Bill,
I have recently seen a number of instances where gold-tin intermetallic compound (IMC) was on the
surface of solder joints but not in the bulk solder. I believe the reason is that the density of
the solid IMC is less than the molten tin-lead and there the IMC floats to the surface prior to
solidification.
Ed Hare
--
SEM Lab, Inc.
Scanning Electron Microscopy and Failure Analysis
Snohomish, WA
(425)335-4400
http://www.sem-lab.com
Bill Fabry wrote:
> Deat "Techies":
>
> I have a "GOLDEN" opportunity for the experts to shine. I have in my possession
> some SMT assemblies built on gold flash fabs that exhibit gold residing on the
> surface of the fillet, rather than being dissolved in the solder. The fillet is
> fully formed with no graininess or other visual anomilies. The phenomenon
> occurs on ONE end of a MELF diode, not on both ends. To answer the obvious
> question, it is NOT dependant on the diode polarity; it happens on either end
> but on one end only.
>
> I have digitally captured a couple of photos of the phenomenon. If you need
> pictorial representation, please e-mail me directly and I can attach it to a
> return e-mail.
>
> As you will see, the gold remains on the surface of the fillet, rather than
> being dissolved in the fillet. A slight scraping of the fillet surface will
> uncover the base solder with NO visual evidence of gold inside. Other
> terminations on other components do NOT exhibit this phenomenon. The assembly
> subcontractor is using standard NO-CLEAN solder paste (OMG Americas 500ADV
> NO-CLEAN 63SN). Unsoldered parts show a tin/lead termination, indicating that
> the gold has possibly migrated over the entire termination.
>
> My question: What mechanism is at work to keep the gold from totally dissolving
> into the Sn/Pb paste after it leaves the fab during reflow?
>
> Thanks for the help.
>
> Bill Fabry, Sr. Manufacturing Engineer
> Plantronics, Inc.
> 345 Encinal Street
> Santa Cruz, Ca. 95060
> (408) 458-7555
>
> [log in to unmask]
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
> ################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|