Ken,
I experienced the same problem years ago. We traced the problem at that time to
gold porosity, allowing oxidation of the nickel. I don't recall the fix , but I
think we went to 50 microinches of electroplated Gold.
I dont know if this helps or not, Good Luck.
Les Connally
> From: Ken Patel <[log in to unmask]>, on 6/24/98 11:54 AM:
> On my electroless Nickel/immersion gold bare-board, I have seen few places
> with brown/copper looking surface. I have following questions in this
> regards.
>
> (1) Is it due to not having Nickel and gold going directly on the copper
> pads?
> (2) What is the reliability risk after the board assembled if above is
> correct
> I mean gold going directly on the copper pads?
> (3) We have specified immersion gold over Nickel. Looking the color which
> is not 100% copper looking, can immersion gold be plated/applied on
> copper or may be process might be changed to electrolytic gold?
>
> re,
> ken patel
> ______________________________________________________
> Ken Patel Phone: (408) 490-6804
> 1708 McCarthy Blvd. Fax: (408) 490-6859
> Milpitas, CA 95035 Beeper: (888) 769-1808
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following
> text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional
> information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or
> 847-509-9700 ext.312
> ################################################################
>
>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|