Milind Rao wrote:
>
> Sorry for my earlier mail without subject
> ------------
> Hi
> We are getting particles in both component holes / via holes on and off
> and in double sided / multilayer boards. This is observed after pattern
> plating
> We use High build copper and Pattern plating.
> In some holes the particles are severe and reduce the hole size
> considerably. The problem is occuring very randomly.
> Has anybody got remedy for this ?
> Thanks in advance for the help
> Milind
>
> ______________________________________________________
> Get Your Private, Free Email at http://www.hotmail.com
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
> For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
> ################################################################
Hello!
I`ve seen a similar probelm. Go to your electroless. Look at the
conditioning step. Feel the side walls of the rinse tank afterwards.
If it`s slippery, well then you might have an algea problem.The algea
get stuck in the holes, gets activated and then plated.
Good luck!
Peter Fogelqvist
Ericsson Circuits
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|