We've seen the same phenomenon as Susan. If I recall, an average thermal
stress can remove up to a ten of a mil of copper from the knee sitting
in the solder pot. We did a lot of work on this when looking into rework
of a multiple segment edge connector. I know of nothing that would
explain significant loss at the top side knee.
Regards,
Paul Terranova
Analytical and Environmental Test Services Lab
Digital Equipment Corporation
200 Forest Street
Mail Stop: MRO3-1/D2
Marlboro, MA 01752-3085
' Phone: (508)467-3109
* Fax: (508)467-6796
* Email: [log in to unmask]
WebSite: http://www.digital.com/lab-services
-----Original Message-----
From: Robisan1 [mailto:[log in to unmask]]
Sent: Sunday, April 26, 1998 10:48 AM
To: [log in to unmask]
Subject: Re: [TN] Dissolution of plated copper
Scott
I have seen this dissolution when performing
multiple thermal stress tests. In fact eventually
knees will disappear completely if you expose
them enough
One thing that can effect this is type of plating
A totally electroless deposit will go into solution
much faster than the electrolytic deposits.
I have done nothing that would compare one to
the other, but I do know it happens
Susan Mansilla
Technical Director
Robisan Lab
################################################################
TechNet E-Mail Forum provided as a free service by IPC
using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to
[log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site
(http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at
[log in to unmask] or 847-509-9700 ext.311
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
################################################################
|
|
|