Hi Mike - Kirkendall voiding is a diffusion phenomena which means time and
temperature are key variables in making the situation better or worst. More
dwell and higher temp's would be the wrong way to go! Get a copy of this
reference:
"The Discovery and Acceptance of the Kirkendall Effect: The Result of a
Short Research Career", H. Nakajima, Journal of Metals, June 1997, page
15-19.
It has an excellent reference section that may be helpful too. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
[log in to unmask] on 03/16/98 03:08:00 PM
Please respond to [log in to unmask]; Please respond to
[log in to unmask]
To: [log in to unmask]
cc: (bcc: David D Hillman/CedarRapids/Collins/Rockwell)
Subject: [TN] How to reduce Kirkendall void?
As I know it, Kirkendall voiding is caused by rapid diffusion of gold
molecules. It was typically related to gold finishes. My question is:
What else can be done to reduce the formation of such void other than
reduce gold thickness?
How about increase dwell time at reflow soldering?
Regards
MIchael Yuen
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional
information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or
847-509-9700 ext.311
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
################################################################
|
|
|