Hi Peter - the ANSIJ-STD-003 is a solderability test specification and not
the solder alloy composition requirements specification. You should be
getting your solder alloy composition requirements from one of two
documents depending on your operation: either ANSIJ-STD-006 or
ANSIJ-STD-001B. A "mix of Sn63/Pb37 and Sn60/Pb40" will be a specific
alloy of solder and not a mixture as inferred. Many technologists would
agree that using the exact eutectic alloy of 61.9 tin-lead (and that is a
debatable value too!) is ideal but in the real world you will get solder
alloy variations as printed wiring assemblies are processed and introduce
small composition changes. Thus having a tolerance (+/- 1%) on the solder
alloy composition is a process practicality. Most PCB customers I am
familiar with use the ANSIJ-STD-006 document or any of the PCB fabrication
specifications with take the ANSIJ-STD-006 values and apply PCB fabrication
tolerances. You can buy the eutectic alloy of 61.9% tin-lead but I
imagine it will be higher in cost than the typical Sn63/Pb37 or Sn60/Pb40.
Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
[log in to unmask] on 01/30/98 08:08:34 AM
Please respond to [log in to unmask]; Please respond to [log in to unmask]
To: [log in to unmask]
cc: (bcc: David D Hillman/CedarRapids/Collins/Rockwell)
Subject: [TN] HASL solder specs
Here are two problems I see with solder standards:
The most exact standard I can find is ANSI/J-STD-003 (1992) which calls out
"plus or minus 1% of nominal". (nominal being 63% tin in a 63/37 bar) Well
what if you change your "nominal" to be a mix of 60/40 and 63/37 to follow
whatever tin concentration happens to be in your HASL pot?
Further: the eutectic composition of tin/lead is 61.9%, which should be
optimal from a wetting perpective. However this 'ideal' concentration is
actually out-of-
spec according to the above standard.
So: what do PCB customers actually require on a finished board?
Peter Blokhuis
Circuits DMA
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional
information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or
847-509-9700 ext.311
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
################################################################
|
|
|