Some things to check:
1) thermal profile - ramp up rate. Your comment re the conductor area
makes this suspicious. Also consider orientation in the oven - does one
side reflow before the other?
2) is the oven running smoothly? (chain or conveyor vibration)
3) pads may be a factor, too much solder can do this. As a crude
experiment you could try removing some of the paste from the pads before
placement.
4) I am assuming you verify the accuracy of the placement before reflow,
but if not it's also a possible problem. Also look at the accuracy of
the screening onto the pads - if your paste is offset to the left and
the part to the right...
** standard disclaimer, opinions are my own, etc.... **
regards,
Graham Collins
Process Engineer,
Litton Systems Limited, Atlantic Division
(902) 873-2000 ext 215
> -----Original Message-----
> From: Gabriela Bogdan [SMTP:[log in to unmask]]
> Sent: Tuesday, October 21, 1997 6:47 PM
> To: [log in to unmask]
> Subject: [TECHNET] Tombstoning
>
> Hello, Technetters!
> I need infomation about Tombstoning of Surface mount components during
> Reflow.
> Does it occure on leadless components in general, disregarding size
> and
> number of connections?
> If so, what are the rules for avoiding it?-Design of pads?
> We encounter a problem which seems to be tombstoning with components
> featuring 3+3 terminations .The corresponding pads on one side are
> connected
> to large conductor areas. The others are not. After reflow many
> components are tipped on one side or misplaced.
> Any suggestions?
> Thank you,
> Gaby
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV
> 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional information.
> For the technical support contact Dmitriy Sklyar at [log in to unmask] or
> 847-509-9700 ext.311
> ##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
##############################################################
|
|
|