Hi tonghh,
You do not say what you want to pretreat Alloy 42 for. I assume it is for
soldering purposes. Be careful!
The industry experience is that there is some Alloy 42 out there (with some
indications that it comes from a mill in South Korea) that is not solderable
no matter what you do to it. Hewlett-Packard-Boise ran into this problem--as
have others, but only HP had the courage and wisdom to be willing to go
public with their problem)--some time ago.
Werner Engelmaier
Engelmaier Associates, Inc.
Electronic Packaging, Interconnection and Reliability Consulting
23 Gunther Street
Mendham, NJ 07945 USA
Phone & Fax: 973-543-2747
E-mail: [log in to unmask]
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
##############################################################
|
|
|