>We are attempting to attach a nickel-plated copper heatsink to a 10
>layer PWB per a set of manufacturing drawings that only states that "the
>heatsink shall be attached with prepreg". It does not call out a
>pressure, temperature, cycle time, or a type of prepreg. We have
>assumed that we would need a "low-flow" type of prepreg. We have tried
>some sample cards with a low-flow prepreg (PC-GF 108V by Westinghouse
>Fortin) that we have on hand; we have had good registration of the
>heatsink to card, but the adhesion has not been as good as we would have
>liked, and the heatsink seems to have been pressed "into" the board (you
>can feel the outline of the heatsink on the backside of the card). We
>ran the press at the lowest possible pressure we can for our press (15
>lbs).
>We are looking for suggestions from anyone who has experience with
>laminating heatsinks to PWBs.
Sounds like too low a pressure for that noflow. The noflow goes bad a little
quicker than normal prepreg too. If you can do vacuum try 75 psi with fresh
noflow; cool in the press. What is the heatsink thickness?
Tom Waznis
Hallmark Circuits Inc., Lam Eng.
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
##############################################################
|
|
|