Hi Christina,
You do not describe what your problem is.
Solder becomes 'brittle' only when it is contaminated with too high a level
of Au or Ag. At smaller quantities, these metals serve to strengthen tin/lead
solder, but in quantity, the brittle and weak AuSn and AgSn intermetallic
compounds dominate physical behavior. Solder also will behave in a
'crystalline' manner at cold temperatures. When subject to creep-fatigue,
solder will develop microcracks along grain boundaries relatively early in
life; these microcracks may give the appearance of 'brittleness' upon
mechanical loading to failure.
I do not know what you mean by 'heat cycle'.
Boards should not be exceeding their Tg during any testing. When you say
'stress testing', what is the purpose of this testing?
Werner Engelmaier
Engelmaier Associates, Inc.
Electronic Packaging, Interconnection and Reliability Consulting
23 Gunther Street
Mendham, NJ 07945 USA
Phone & Fax: 973-543-2747
E-mail: [log in to unmask]
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
##############################################################
|
|
|