Subj: Re: FAB: Re: Pink ring and hard failures
Date: 97-07-19 15:50:27 EDT
From: Rwmpc
To: [log in to unmask]
OK Technetters - Here's another one to think about. If you run boards
through the line and leave them in acid copper WITHOUT plating current, even
for the full duration of a typical plating cycle, you may see some attack
and/or what looks like pink ring formation. Even the creation of a small
"wedge".
Take another load of boards and run as you normally would, with current
applied by ramp-up, going in hot or whatever, and you'll see pink ring within
minutes. Sort of leads you to believe that the oxide dissolution, while it
is chemical, is markedly accelerated by electrolysis.
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
|
|
|