Received: |
by ipc.org (Smail3.1.28.1 #2)
id m0wXSW5-000BjPC; Fri, 30 May 97 09:18 CDT |
Encoding: |
90 Text |
Old-Return-Path: |
|
Date: |
Fri, 30 May 97 06:38:05 cst |
Precedence: |
list |
Resent-From: |
|
Resent-Sender: |
|
X-Status: |
|
Status: |
O |
X-Mailing-List: |
|
>From bergdi Fri May 30 09: |
19:17 1997 |
TO: |
|
Return-Path: |
<TechNet-request> |
Resent-Message-ID: |
<"uy2hW2.0.BiL.-4kZp"@ipc> |
Subject: |
|
From: |
|
X-Loop: |
|
Cc: |
|
From [log in to unmask] Mon Jun 2 09: |
05:57 1997 |
Message-Id: |
|
Parts/Attachments: |
|
|
Hi Werner!
I agree with your assessment/description of the solderability
degradation for a thin solder finish but I think that you are giving
the Pb oxide too much credit as a contributing underlying mechanism.
Published data within the last 2 years has shown that Pb oxide is
present in only small volume/area in comparison to Sn oxide or CuxSnx
intermetallic oxide. The Sn and/or CuxSnx oxides dominate the
wettability causing the solderability problems with the increased
liquidus temperature issues of the Pb rich layer being a bigger
contributor than any Pb oxide issues. HASL finishes are definitely
headaches if good process controls are not followed and maintained.
Dave Hillman
Rockwell Collins
[log in to unmask]
______________________________ Reply Separator _________________________________
Subject: Re: RE: IPC A 600 E:vert hasl
Author: [log in to unmask] at ccmgw1
Date: 5/29/97 2:03 PM
Hi Frank,
You responded to my message of:
>>Be careful about thin HASL solder layers; below 5 micro-meters (200
>>micro-inches) solderability can decrease rapidly with shelf life.
with a message dated 05/27/97 11:31:19, [log in to unmask] (frp) :
>I once read about a study in which the shelf life of 1 year was >simulated
by a baking process. Then the grow of the intermetallic layer >Cu/PbSn was
measured. The outcome of this investigation was that the >intermetallic
layer increased by 0.8 microns. So to have a good >solderability after
storage 1 year
>(normal conditions) you only need a minimum of 1 micron of PBSn.
>So I don't think that having less than 5 microns will give problems as
>long as it is not below 1 micron.
>
>Kind regards
>Frank Petit
I was perhaps too brief in my response--I would wish things were quite that
simple. I have clients that wound up with non-solderable soldering pads
specing a minimum of 0.1 mils (2.5 microns) of HASL coating thickness,
whereas specing 5 microns eliminated the problem. While IMC growth at low
temperatures, like 20 C, are indeed slow, it rapidly increases with
increasing temperature. While it takes about 1 year to grow 0.8 microns of
IMC at room temperature, the same thickness is obtained in about 3 weeks at
40 C.
It is also a matter of solder composition; the higher the Sn content the
faster the IMC growth.
Further, one has to consider what the HASL layer actually consists of. The
copper pad is covered by (1) a thin layer of Cu3Sn IMC which in turn is
covered by (2) a thicker Cu6Sn5 IMC layer, which is the layer that grows;
adjacent to the Cu6Sn5 layer is (3) a layer from which the Sn has been
depleted to form the IMC layers (this layer has a higher Liquidus temperature
because of the higher lead content); this layer is (hopefully) covered with
(4) a layer of the regular solder, which in turn is covered with (5) a layer
containing non-solderable lead oxides. If the HASL process removes too much
solder, the solder layer (4) becomes very thin or non-existent. The solder lay
er (4) with its low Liquidus temperature is required during reflow soldering
to break up the Pb oxide layer (5) as well to help liquify the Pb-rich layer
(3).
Colin Lea's book 'A Scientific guide to Surface Mount Technology is a good
source for more detailed information.
Therefore, a total HASL layer thickness of 2 microns or less is sure to get
you in trouble unless you have a perfect JIT capability.
Werner Engelmaier
Engelmaier Associates, Inc.
Electronic Packaging, Interconnection and Reliability Consulting
23 Gunther Street
Mendham, NJ 07945 USA
Phone & Fax: 201-543-2747
E-mail: [log in to unmask]
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
|
|
|