TECHNET Archives

May 1997

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Received:
by ipc.org (Smail3.1.28.1 #2) id m0wWVh5-000BisC; Tue, 27 May 97 18:30 CDT
From [log in to unmask] Wed May 28 08:
16:15 1997
Old-Return-Path:
Date:
Tue, 27 May 1997 19:40:26 -0400 (EDT)
Precedence:
list
Resent-From:
Message-ID:
X-Status:
Status:
O
X-Mailing-List:
<[log in to unmask]> archive/latest/12953
TO:
Return-Path:
<TechNet-request>
>From bergdi Tue May 27 18:
30:39 1997
Resent-Message-ID:
<"PHVAF2.0.e17.AwsYp"@ipc>
Subject:
From:
X-Loop:
Resent-Sender:
TechNet-request [log in to unmask]
Parts/Attachments:
text/plain (32 lines)
Jim, 

If the resin recession is in zone B (para 3.6.2.3) it would be by definition
a laminate void and the rules for a laminate void would apply.  The evaluator
cannot determine how it was produced and could not determine if it existed
prior to solder floating.

I think you artificially created resin recession on the power plane by
dipping it 6 times for 10 seconds.  IPC-6012 states that you evaluate for for
resin recession after solder floating the coupon one time on the solder pot.
 If you do test sequences that are not per the test method designated in
IPC-6012 you may produce different results and the final characteristics may
not fall within the acceptability criteria shown in IPC-6012.  For example,
other test temperatures such as 371 deg C (700 deg. F) which are popular with
some users do not produce acceptable results with all materials; therefore
special conditions must be agreed on by the user and supplier.  This is what
is generally stated in IPC-6011 and would be part of the "Procurement
Documentation".     

Phil Hinton

***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]>   *
* with <subject: subscribe/unsubscribe> and no text in the body.          *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact   *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask]      *
***************************************************************************


ATOM RSS1 RSS2