Mime-Version: |
1.0 |
From [log in to unmask] Wed Apr 16 10: |
15:02 1997 |
Old-Return-Path: |
|
Date: |
Wed, 16 Apr 1997 02:10:21 +0100 |
Precedence: |
list |
Resent-From: |
|
Resent-Sender: |
|
X-Status: |
|
Status: |
O |
X-Mailing-List: |
|
X-Sender: |
|
TO: |
|
Return-Path: |
<TechNet-request> |
X-Loop: |
|
Received: |
by ipc.org (Smail3.1.28.1 #2)
id m0wHI6L-000BjcC; Tue, 15 Apr 97 18:57 CDT |
Resent-Message-ID: |
<"UzlmX.0.AYL.dN1Lp"@ipc> |
Subject: |
|
From: |
|
Content-Type: |
text/plain; charset="us-ascii" |
Cc: |
|
X-Mailer: |
Windows Eudora Light Versión 1.5.2 |
Message-Id: |
|
Parts/Attachments: |
|
|
At 16:27 14/04/97 EDT, you wrote:
>All
> My customer is designing a board with a bonded aluminum heatsink of .062
>aluminum on the component side. ie as if it were a copper pour zone on the
>board. Has anybody any experience with SMT reflow on a board like this?
>
>Peter Roy
>Toronto
>
>=========================================
dear friend,
you can use any standard alloy with Zinc (4 or 4,5% of Zn)
If normally you are using Tin lead alloys, with aluminium, probably, it will
appears the called BATTERY EFFECT (corrosion in solders).
If you wish to solder with Sn Pb alloys, you need to prepare the surface
with an electrolitic process that is recover the aluminium with Cu (cooper)
and after re-recover the Cu with Cr (Chrome).
Good look
=============
ANTONI CHERTA
(Barcelona)
Ph:+34.07.20.49.42
Fx:+34.3.274.00.80
E-mail: [log in to unmask]
=====================
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
|
|
|