Elizabeth:
>From the limited data that you have provided, I would say that the problem
here is that the flux has dried out prior to the wave or that the flux has
not been applied at all in the areas that look bad.
The solder pot temperature of 500?F is acceptable. The topside board
temperature of 210? - 220?F also is within normal limits but, it is on the
high side. I would suggest that your customer either turn up the conveyor
speed or turn down the pre-heat to the extent that the topside temperature
would be between 180? - 200?F. In addition, I would make sure the board is
being adequately fluxed.
Bill Kasprzak
Moog Inc.
(716)652-2000 ext. 2507
[log in to unmask]
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
|
|
|