Received: |
by ipc.org (Smail3.1.28.1 #2)
id m0vPVF4-0000SBC; Mon, 18 Nov 96 09:04 CST |
Old-Return-Path: |
|
Date: |
18 Nov 1996 09:12:55 -0600 |
X-Status: |
|
Precedence: |
list |
Resent-From: |
|
Conversion: |
Allowed |
Disclose-Recipients: |
Prohibited |
Resent-Sender: |
|
MIME-Version: |
1.0 |
Status: |
O |
Priority: |
normal |
X-Loop: |
|
X-Mailing-List: |
|
Content-Return: |
Allowed |
X400-MTS-Identifier: |
[/c=US/admd=MCI/prmd=Honeywell/; 06A4932907CF74DF-HW-MTA-AZ] |
TO: |
|
X400-Originator: |
|
Original-Encoded-Information-Types: |
IA5-Text |
From [log in to unmask] Mon Nov 18 10: |
55:51 1996 |
X400-Recipients: |
non-disclosure; |
Alternate-Recipient: |
Allowed |
Message-Id: |
<06A4932907CF74DF*/c=US/admd=MCI/prmd=Honeywell/o=AZ-MTA/ou=MSMail/ou=CAS/s=Edwards/g=Ted/i=A/@MHS> |
Resent-Message-ID: |
<"rccxk2.0.XDH.eh7ao"@ipc> |
Subject: |
|
From: |
|
Return-Path: |
<TechNet-request> |
X400-Received: |
by /c=US/admd=MCI/prmd=Honeywell/; converted ( IA5-Text);
Relayed; 18 Nov 1996 09:12:55 -0600
by mta HW-MTA-AZ in /c=US/admd=MCI/prmd=Honeywell/; converted (
IA5-Text); Relayed; 18 Nov 1996 09:12:55 -0600 |
X400-Content-Type: |
P2-1988 ( 22 ) |
Content-Identifier: |
06A4932907CF74DF |
Parts/Attachments: |
|
|
Sounds like you have interplane separation. It is a separation of the
plated copper on the hole wall from the edge of the inner layer. Dr. Alan
Poskanzer wrote an article in Plating and Surface Finishing for March 1990
that you might want to read. It's title is IP Separation: Its Causes and
Cures. The magazine is by the American Electroplaters Society. Since we
are on the subject, I'd like to piggyback on this and ask: Is anyone seeing
post separation of the Tg 170 range materials and if so do you have a root
cause?
----------
From: [log in to unmask]
To: [log in to unmask]
Subject: Interconnect Failure
Date: Monday, November 18, 1996 8:17AM
RECENTLY WE FIND INNER LAYER OPEN COMPLAINT IN EIGHT LAYER BOARDS FOR ONE
PARTICULAR PART NUMBER. ON MICRO SECTIONING WE FIND NO INTER CONNECTION
BETWEEN HOLE COPPER AND INNER LAYER (SEVENTH LAYER).
THE CONSTRUCTION 1,2,7 & 8 ARE SIGNAL LAYERS REST ARE GROUND LAYERS.
TWO TO SEVEN ( INNER LAYERS HAVE ONE OUNCE BASE COPPER) ONE AND EIGHTTH
LAYER
HALF OUNCE BASE COPPER.
COPPER INSIDE THE HOLES IS >25 MICRONS. WE DONT FIND ANY WEDGE VOID OR
PINK RING.
THE CUSTOMER BAKES THE BOARD BEFORE ASSEMBLY AND ALL BOARDS PASSED
ELECTRICAL TESTING. BUT AFTER ASSEMBLY THE CUSTOMER REPORTS INNER LAYER
OPEN.
CAN ANYONE THROW LIGHT ON THE ABOVE PROBLEM?
Thanks in advance
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To unsubscribe from this list at any time, send a message to: *
* [log in to unmask] with <subject: unsubscribe> and no text. *
***************************************************************************
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To unsubscribe from this list at any time, send a message to: *
* [log in to unmask] with <subject: unsubscribe> and no text. *
***************************************************************************
|
|
|