Steve,
From the drying rate I have seen for dry oven usage I would think no temperature is required for reel of parts. The diffusion distances are so small. Just don't put them in sealed bags and expect a quick dry!
I did some little experiments with drying single PCBs in poly bags, it can take days to diffuse out through the poly. I see people put packs of PCBs into dry boxes while the PCBs are still in sealed poly bags. Worse yet I sometime see PCBs being "Dried" while in moisture proof bags. Wow that makes a lot of sense.
Poly is ok for a few weeks if you include desiccants. But diffusing through long stretches of FR4 I don't know about.
The other unresolved question is a PCB with metal power planes. The planes of copper do a great job of sealing in any moisture into inside prepreg. I asked some fab guys out at Apex and most were not sure. One guy said internal layers should be dry as the lamination presses are hot and provide vacuum. But even there the copper foils are still like hermetic seals, I think.
Does anyone really know something? (IE no "It Depends" 😊 )
Bob K.
-----Original Message-----
From: TechNet <[log in to unmask]> On Behalf Of Steve Gregory
Sent: Monday, April 16, 2018 10:20 AM
To: [log in to unmask]
Subject: Re: [TN] Vacuum Baking
Hi All,
I know this thread is about vacuum baking, but I would like to ask about baking components on tape and reel, I have not actually done this. I remember seeing discussion about the topic on Technet, but I can't remember all the details.
I know when I ask what temperature is safe to bake tape and reel components "it depends" will come up, it probably depends on what kind of carrier tape on top film cover tape is used, is it pressure sensitive adhesive or heat seal cover tape? I'm seeing a need that may require more baking of reeled components now for some reason.
Is it just me, or does it seem that more and more components are being designated as MSL 2A and higher lately?
Steve
On Mon, Apr 16, 2018 at 8:09 AM, Yuan-chia Joyce Koo < <mailto:[log in to unmask]> [log in to unmask]>
wrote:
> you can make board vertical stand in the PWA carrier tray with slot.
> you need surface area for moisture to escape...assume you use low
> temperature in vacuum baking, little warpage would happen unless it
> is very thin large size board.
> On Apr 16, 2018, at 9:23 AM, Robert Kondner wrote:
>
> Hi,
>>
>> If you have a stack of PCBs, lets say 25 or 50 boards which is a
>> stack 2 or 3 inches high, can water vapor diffuse out the space between the boards?
>> Does laying a thick tissue between the boards help or is it best to
>> place each board in edge supported carriers? I worry about warp if a
>> board is edge supported while at elevated temps.
>>
>> Does anyone has knowledge here or even an educated guess?
>>
>> Thanks,
>> Bob K.
>>
>> -----Original Message-----
>> From: TechNet < <mailto:[log in to unmask]> [log in to unmask]> On Behalf Of David Hillman
>> Sent: Monday, April 16, 2018 8:11 AM
>> To: <mailto:[log in to unmask]> [log in to unmask]
>> Subject: Re: [TN] Vacuum Baking
>>
>> Hi folks - we did some vacuum baking experimentation a few years back
>> and yes, vacuum baking can be effective but it is not as straight
>> forward as you would imagine. You need to carefully select the vacuum
>> bake parameters or you will actually impede water diffusion. You can
>> cause ice formation rather than water evaporation depending on your
>> parameters (put a shallow pan of water in a vacuum chamber and try
>> it, its kinda fun). Wayne's approach is much simpler and far more
>> practical/effective in terms of moisture removal.
>>
>> Dave Hillman
>> Rockwell Collins
>> <mailto:[log in to unmask]> [log in to unmask]
>>
>>
>> On Sun, Apr 15, 2018 at 11:43 AM, Wayne Showers <
>> <mailto:[log in to unmask]> [log in to unmask]> wrote:
>>
>> The problem with vacuum drying is not so much the boiling point of
>>> water as in an unimpeded environment, those values are: At 25" Hg :
>>> 56C, 27" Hg :
>>> 45C, 28" Hg :40C, and so on. The problem is degree of impediment
>>> caused by the actual plastic. To build off what Yuan-chia Joyce Koo
>>> has stated but with a different vector in mind, the plastic material
>>> of moisture bags for instance is highly resistant to diffusion.
>>> Different polymers will follow accordingly.
>>>
>>> For information, many plastics must be dried immediately prior to
>>> molding otherwise they suck up moisture like a sponge. Common
>>> hygroscopic polymers are Nylon, ABS (Acetyl Butyl Styrene), PC
>>> (Polycarbonate), and PMMA (Poly (methyl methacrylate)). Nylon and
>>> PMMA are very common materials in component shells. ABS and PC
>>> index* at temperatures not much higher than boiling water and are
>>> not typically used. PP (Polypropylene) and PE
>>> (Polyethylene) are not so bad, hence their use in capacitors, but
>>> these index in the 200C range making them a bear for SMT placement.
>>> My general rule is the higher the MSL number, i.e., the more likely
>>> a part is to absorb moisture, the easier it is to dry.
>>>
>>> For normal bake (NO vacuum), here is the formula I derived several
>>> years
>>> ago:
>>> Thickness (mm) X Thickness (mm) (Divided by) Bake Temp Factor
>>> D125oC=
>>> 0.4427 // D90oC= 0.1270 // D40oC= 0.0131, Result is time in hours.
>>>
>>> I have never experimented with Vacuum Acceleration, but I will query
>>> the Penn State Plastics Engineering group with what we are trying to
>>> resolve and post those results to the J-STD-033 committee as well as
>>> here.
>>> * Index is the temperature at which a plastic flows well enough to
>>> be molded. It is neither solid nor liquid, but soliquid.
>>>
>>> This all sounds like a job for Clumpy and Kloumpios when they are
>>> next available.
>>>
>>>
--
Steve Gregory
Kimco Design and Manufacturing
Process Engineer
(208) 322-0500 Ext. -3133
--
This email and any attachments are only for use by the intended
recipient(s) and may contain legally privileged, confidential, proprietary or otherwise private information. Any unauthorized use, reproduction, dissemination, distribution or other disclosure of the contents of this e-mail or its attachments is strictly prohibited. If you have received this email in error, please notify the sender immediately and delete the original.
|