TECHNET Archives

October 2017

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
John Burke <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Thu, 19 Oct 2017 02:31:43 +0000
Content-Type:
text/plain
Parts/Attachments:
text/plain (38 lines)
	




You need to consider some factors here - You state that the pads have vias.
1  ANY pad lift must have stressed the via OR the via has stressed the PAD2 Is the via stacked onto a core via and if so what is the CTE above glass transition of the filler material?3 What is the cool down slope on the reflow? In this case fast is never good.


John Burke

_____________________________
From: Zilber Gil <[log in to unmask]>
Sent: Wednesday, October 18, 2017 10:23 PM
Subject: [TN] Pad lifting or lifted land
To: <[log in to unmask]>


Fellow TechNetters:

I have a problem of lifted land (via`s pad) after reflow. More the 90% of the pads show it on both sides of the PCB (Vias are filled and cap plating).
According to IPC lifted land after thermal stress is allowed.
In many cases, a conductor is connected to these pads and in this case, the reliability of the connected area to the lifted pad is probably very poor (most of the PCBS worked after the assembly, but one show discontinuity. Many vias are under BGAs connected as a dog bone to the BGA pads).
I contacted the manufacturer and he told me that the PCBs are ok according to IPC thus they will not compensate us.


Now I have a few questions:
1. IPC did not mention any conductor connected to these pads, why? What about reliability issues in this case (obviously poor?)?
2. Do I have any case against the manufacturer?
3. At IPC 6012 and Mil-prf-55110 lifted land refer to the pad of the vias, but it is not verbally written. It is showed on the pictures (at the MIL). Thus, one can interpret that lifted land, i.e. component pad, can be lifted from the board and it is acceptable...?? (imagine a BGA "jumping" up and down during vibration... :)
4. After that issue, I am going to change our spec and not allowed any lifted land (before or after thermal stress).

Thank you for your inputs,

Gil Zilber
Elta Systems Ltd.
The information contained in this communication is proprietary to Israel Aerospace Industries Ltd. and/or third parties, may contain confidential or privileged information, and is intended only for the use of the intended addressee thereof. If you are not the intended addressee, please be aware that any use, disclosure, distribution and/or copying of this communication is strictly prohibited. If you receive this communication in error, please notify the sender immediately and delete it from your computer.