Subject: | |
From: | |
Reply To: | |
Date: | Thu, 13 Jul 2017 20:11:56 +0000 |
Content-Type: | text/plain |
Parts/Attachments: |
|
|
Here's my thoughts:
(a) use fresh chemicals.
(b) If you are using 30% NH4OH, cut back on the DI H2O.
(c) once mixed, this etchant has a short shelf life (several hours at best)
I use 25 ml of NH4OH (50%), 25 ml DI H2O and about 0.5 ml H2O2 (3%).
Are you etching PCB copper or solid Cu slugs?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of [log in to unmask]
Sent: Thursday, July 13, 2017 2:44 PM
To: [log in to unmask]
Subject: Re: [TN] 1:1:1 Copper Etchant, Delineation Region of copper plating interface
Dell - Internal Use - Confidential
That's the whole problem...... I only have the listed chemicals to work with........
Victor,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Tony Lentz
Sent: Thursday, July 13, 2017 2:37 PM
To: [log in to unmask]
Subject: Re: [TN] 1:1:1 Copper Etchant, Delineation Region of copper plating interface
Hello Victor,
Increasing the concentration of the hydrogen peroxide will make this solution more aggressive as a copper etchant. The ammonium hydroxide is mainly there to aid in keeping the copper dissolved as a copper ammonium ion.
Best regards,
Tony Lentz
Chemist / Field Application
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of [log in to unmask]
Sent: Thursday, July 13, 2017 1:17 PM
To: [log in to unmask]
Subject: [TN] 1:1:1 Copper Etchant, Delineation Region of copper plating interface
Fellow TechNetters:
Is there any possible way to make the above stated etchant STRONGER/AGGRESSIVE: Here are the chemicals: Perhaps by varying the volume of one of the three constituents.
1 - Ammonium Hydroxide, 28.0 - 30.0%
1 - Hydrogen Peroxide, 3%
1 - Deionized water
Victor,
|
|
|