Hi Gil - you hit on one of my soapbox topics so I have respond! What data
source are you citing that shows 6 micrometers of IMC results in solder
joint failure? And for the IMC, is it the Cu3Sn or the Cu6SN5 phase? The
industry is constantly "reminded" that thick IMC is brittle and will cause
a loss of solder joint integrity but where is the data? Everyone is in
consensus that IMC phases have been shown to have brittle properties but
when I push for hard data/investigations/studies, demonstrating failures
due to excessive, thick IMC phase, the real root cause has always turned
out to be an out of control or excessive, abusive soldering process -
typically a soldering process most folks would say "ohh, I wouldn't do
that with my soldering process". For a dwell temperature of 100C, I will
grow approximately 5 micrometers of IMC ( combine Cu3Sn and Cu6Sn5 phases)
in 1660 hours using the standard IMC equations for tin over copper (my
calculations don't match the details you listed). There are multiple
examples of electronic products in many different product use environments
that easily exceed that time and operate at that temperature yet we don't
see reports of product integrity data. Unless you have some nontypical
variable for your product in its use environment (basically, a variation of
Doug saying "it depends" but with less gray area), I don't believe you have
a solder joint integrity concern. Don't get me wrong, I think its great
that folks are looking at how much IMC phase is produced/found on their
solder joints but I think we overstate the topic on most occasions.
Dave Hillman
Rockwell Collins
[log in to unmask]
On Thu, May 19, 2016 at 7:34 AM, Zilber Gil <[log in to unmask]> wrote:
> Hello Technet`s,
>
> As we know above 6 micrometers of intermetallic (CuSn) could cause failure
> due to brittle structure of the intermetallic. I found in some experiment
> that at 100 deg C after 32 days the intermetallic (CuSn from Sn-40Pb) grow
> in about 6 micron. Is it true? What should I do if the board should see 100
> deg C for long time and what about >=90 dig?
>
> Thanks,
>
> Dr. Gil Zilber
> Technologiest
> Elta Systems Ltd.
>
> The information contained in this communication is proprietary to Israel
> Aerospace Industries Ltd. and/or third parties, may contain confidential or
> privileged information, and is intended only for the use of the intended
> addressee thereof. If you are not the intended addressee, please be aware
> that any use, disclosure, distribution and/or copying of this communication
> is strictly prohibited. If you receive this communication in error, please
> notify the sender immediately and delete it from your computer.
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|