Hi Steve - we need the Technet board subject matter experts help on this
but having that much electrical potential would certainly make for having
possible corrosion issues and failure modes (such as CAF) if the board
fabrication was not done correctly. There also could be a design rule
violation such as that dielectric layer being too thin - ok TechNet board
folks - thoughts?
Dave
On Fri, Apr 8, 2016 at 11:44 AM, Steve Gregory <[log in to unmask]> wrote:
> Hi again Dave,
>
> So the PCB is a .090" thick, 8-layer board, the stack-up is this:
>
> Soldermask
> Layer 1
> ----------
> Ground
> ----------Pre-preg
> Layer 3
> ----------
> +12V
> ----------Pre-preg
> -12V
> ----------
> Layer 6
> ----------Pre-preg
> Ground
> ----------
> Layer 8
> Soldermask
>
> Steve
>
>
> On Fri, Apr 8, 2016 at 10:18 AM, David Hillman <
> [log in to unmask]> wrote:
>
>> Hi Steve - yes, you have enough physical details that a lab that
>> routinely conducts FA work on electronic assemblies (there are several who
>> are part of Technet) would have a reasonable chance of finding the root
>> cause. At a very minimum with the details you have on this issue, the
>> laboratory should be able to rule out possible root causes even if they
>> can't find a specific root cause. I didn't see any dendritic shorting - is
>> the belief that the shorting is internal to the pwb?
>>
>> Dave Hillman
>> Rockwell Collins
>> [log in to unmask]
>>
>>
>> On Fri, Apr 8, 2016 at 11:00 AM, Steve Gregory <[log in to unmask]>
>> wrote:
>>
>>> Good Morning All,
>>>
>>> We have an assembly that we build here for a customer that we built for
>>> some time, over 2,000 assemblies. There have been some failures that our
>>> customer has had field returns with that are beginning to escalate. There
>>> have been 12 field failures that we know of. The failures are avionic
>>> assemblies that have been in the field ranging from 111 days to 472 days.
>>> The actual failures are internal +12V to -12V shorts and we need to know
>>> why. I have two failed assemblies here. Here are a couple of external
>>> photos of a via that shows the short:
>>>
>>> http://stevezeva.homestead.com/Internal_Short.jpg
>>>
>>> http://stevezeva.homestead.com/Internal_Short_Close.jpg
>>>
>>> So my question is, can a lab take these boards and examine them to
>>> determine what the root cause actually is from the two assemblies that I
>>> have, or does there need to be more samples? What is the range we should
>>> expect to pay for this type of analysis?
>>>
>>> We're trying to work with our PCB vendor on this issue, but I have also
>>> been asked by my boss to pursue this with a third party.
>>>
>>> Thanks!
>>>
>>> Steve
>>>
>>>
>>> ______________________________________________________________________
>>> This email has been scanned by the Symantec Email Security.cloud service.
>>> For more information please contact helpdesk at x2960 or
>>> [log in to unmask]
>>> ______________________________________________________________________
>>> --
>>>
>>>
>>> This email and any attachments are only for use by the intended
>>> recipient(s) and may contain legally privileged, confidential,
>>> proprietary
>>> or otherwise private information. Any unauthorized use, reproduction,
>>> dissemination, distribution or other disclosure of the contents of this
>>> e-mail or its attachments is strictly prohibited. If you have received
>>> this
>>> email in error, please notify the sender immediately and delete the
>>> original.
>>>
>>
>>
>
>
> This email and any attachments are only for use by the intended
> recipient(s) and may contain legally privileged, confidential, proprietary
> or otherwise private information. Any unauthorized use, reproduction,
> dissemination, distribution or other disclosure of the contents of this
> e-mail or its attachments is strictly prohibited. If you have received this
> email in error, please notify the sender immediately and delete the
> original.
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|