Bob,
Here's what I know by looking at the Sn-Ni (the k type t/c is loaded
with Ni) alloy phase diagram, around 231C which is the invariant
transformation temperature for liquid to Ni3Sn4 bimetallic transition
alloy, the composition of the thermocouple junction changes. This
shifts in the expected temperature v/s e.m.f. characteristics or loss
of functionality. I will read the document, thanks.
Bhanu
On Tue, Mar 8, 2016 at 11:48 AM, Robert Kondner
<[log in to unmask]> wrote:
> Bhanu,
>
>
>
> You gotta read a book on this. See:
> http://www.pyromation.com/Downloads/Doc/Training_TC_Theory.pdf
>
>
>
>
>
> Myth: There should never be a third metal in the hot junction
>
>
>
> To create a thermocouple junction, all that is needed is to electrically
> short the ends together. Butting the wire ends against a metal surface will
> create a junction. Remember, that the thermocouple signal is generated over
> the entire length of wire.
>
>
>
> Lets say you have two side of the thermocouple, side A and side B and
> another material C.
>
>
>
> The welding of side A to a material C results in a thermocouple being
> formed, The welding of side B to the material forms another thermocouple.
> The final sum of the two thermocouples equals the junction potential of A
> welded to B.
>
>
>
> Tell me if I am wrong! Been known to happen!
>
>
>
> Bob K.
>
>
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Bhanu Sood
> Sent: Tuesday, March 08, 2016 10:59 AM
> To: [log in to unmask]
> Subject: Re: [TN] Soldering a K Type TCouple to FR4 Board
>
>
>
> If you weld each side to a third material, its no longer a junction, no
> thermo-"couple"..
>
>
>
> On Tue, Mar 8, 2016 at 10:54 AM, Robert Kondner <[log in to unmask]>
> wrote:
>
>> Hi,
>
>>
>
>> I do not think this is correct.
>
>>
>
>> My recollection of the physics is you can cut the bead off the
>> thermocouple, weld each side to a 3rd material, and get the temperature of
>> the material.
>
>>
>
>> What this does is introduce additional junctions but the final output is
>> always equal to the characteristics of the original bead. Even if you manage
>> to diffuse other materials into the thermocouple wire materials it is the
>> same case.
>
>>
>
>> Anyone else out there have any thoughts?
>
>>
>
>> Bob K.
>
>>
>
>> -----Original Message-----
>
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Bhanu Sood
>
>> Sent: Tuesday, March 08, 2016 8:43 AM
>
>> To: [log in to unmask]
>
>> Subject: Re: [TN] Soldering a K Type TCouple to FR4 Board
>
>>
>
>> Are you sticking the thermocouple head in SAC solder? Be careful!
>
>>
>
>> Once you stick the t/c in SAC solder and melt to 250C (which bwt is
>
>> above the 185C curie point) the chromel which contains 90-percent
>
>> nickel and 10-percent chromium and alumel which contains approximately
>
>> 95 percent nickel, with aluminum, silicon, and manganese making up the
>> other 5 percent will alloy with the tin, changing the temperature e.m.f
>> relationship. You may not have a working thermocouple afterwards.
>
>>
>
>>
>
>> On Tue, Mar 8, 2016 at 8:14 AM, Bob Wettermann <[log in to unmask]> wrote:
>
>>> Morning All:
>
>>>
>
>>> Has anyone had success in soldering Type K Thermocouples to a PCB.
>
>>> The assembly call for a SAC305 no clean alloy....
>
>>>
>
>>> There are 2 THole connections that will need to be hand-soldered as
>
>>> part of this assembly.
>
>>>
>
>>> Thanks!
>
>>>
>
>>>
>
>>> _____________________________________________________________________
>
>>> _ This email has been scanned by the Symantec Email Security.cloud
>
>>> service.
>
>>> For more information please contact helpdesk at x2960 or
>
>>> [log in to unmask]
>
>>> _____________________________________________________________________
>
>>> _
>
>>> --
>
>>> Bob Wettermann
>
>>> BEST Inc
>
>>> [log in to unmask]
>
>>> Cell: 847-767-5745
>
>>
>
>>
>
>>
>
>> --
>
>> Bhanu Sood
>
>> Tel: (202) 468-8449
>
>>
>
>> ______________________________________________________________________
>
>> This email has been scanned by the Symantec Email Security.cloud service.
>
>> For more information please contact helpdesk at x2960 or
>
>> [log in to unmask]
>
>> ______________________________________________________________________
>
>>
>
>
>
>
>
>
>
> --
>
> Bhanu Sood
>
> Tel: (202) 468-8449
>
>
>
> ______________________________________________________________________
>
> This email has been scanned by the Symantec Email Security.cloud service.
>
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
--
Bhanu Sood
Tel: (202) 468-8449
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|