TECHNET Archives

December 2015

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, 'Grossmann, Günter' <[log in to unmask]>
Date:
Mon, 14 Dec 2015 08:17:23 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Bev Christian <[log in to unmask]>
Message-ID:
Subject:
From:
Bev Christian <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="UTF-8"
MIME-Version:
1.0
Parts/Attachments:
text/plain (112 lines)
I agree with Günter.  It would be more problematic if one were talking about a high humidity test where the power died such that your samples went through the dew point while under electric potential.  In that case I would restart the test and if all samples passed then then all is good, but if they failed, then I would repeat the test.  Coming back to your thermal cycling test, if you wanted to get really picky, you might want to consider adding one or two more cycles to the total.   :)

Regards,
Bev 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Grossmann, Günter
Sent: December 14, 2015 5:45 AM
To: [log in to unmask]
Subject: [TN] AW: [TN] Query on Temperature Cycling testing

We do a lot of thermal cycling tests and quite often we have to remove the samples from the chamber for optical evaluation. The aim of the thermal cycles is to induce mechanical load due to the mismatch of the coefficients of thermal expansion. Because of the plasticity of the materials used in electronic applications low cycle fatigue will be activated as the dominant failure mechanism. In low cycle fatigue the sum of the cyclic plastic stain is the parameter which degrades the material and thus it is not necessary to run the test continuously in my opinion.

Best regards

Günter Grossmann
Scientist
Empa
Swiss Federal Laboratories for Materials Science and Technology Überlandstrasse 129
8600 Dübendorf
Switzerland
Tel +41 58 765  4279
Fax +41 58 765 6954
[log in to unmask]
www.empa.ch

Diese Mitteilung ist ausschliesslich für die als Empfänger aufgeführte Person(en) oder Firma bestimmt. Sie kann persönliche und/oder vertrauliche Informationen enthalten. Sollten Sie diese Mitteilung irrtümlicherweise erhalten haben, bitten wir Sie, uns umgehend per E-Mail zu informieren, sämtliche Ausdrucke zu vernichten und die E-Mail-Dateien zu löschen.
This message is intended for the exclusive use of the individual(s) or entity to whom it is addressed. It may contain information that is privileged and/or confidential. Should you have received this message erroneously, please notify us immediately by e-mail, destroy any printouts and delete all electronic files contained in this message.

> -----Ursprüngliche Nachricht-----
> Von: TechNet [mailto:[log in to unmask]] Im Auftrag von colin mcvean
> Gesendet: Sonntag, 13. Dezember 2015 10:55
> An: [log in to unmask]
> Betreff: Re: [TN] Query on Temperature Cycling testing
> 
> Namaste Nagaraj,
> In my opinion, the condition for the test is that it should be 
> continuous and any significant break in the test which allows for the 
> parts under test to 'normalize' will invalidate the test result. As 
> its a customer qualification if I was themI would have reservations 
> about how reliable the product performed given such a break. 
> Personally I would scrap the samples and repeat the test with fresh 
> product. RegardsColin
> 
> 
> Sent from Yahoo Mail for iPhone
> 
> 
> On Sunday, December 13, 2015, 4:59 pm, Nagaraj U 
> <[log in to unmask]> wrote:
> 
> Hi All,
> 
> We are manufacturers of bare PCBs.
> 
> We were conducting temperature cycling test as per Condition B of 
> JESD22- A104D (-55°C to +125°C). The test requirement was for 500 
> cycles. This testing was a part of qualification of PCBs for one of our customer.
> 
> We have loaded a set of 4 bare PCBs and 4 assembled PCBs (not powered 
> on
> - loaded in passive mode after assembly) in the thermal cycling chamber.
> 
> Now, 350 cycles are completed, but the thermal cycling chamber has 
> stopped due to some issue with the thermal cycling equipment.
> 
> Now my question......... can the testing be continued for another 150 
> cycles to complete 500 cycles OR should the whole exercise be started 
> from fabrication of fresh PCBs, Assembly and do the temperature 
> cycling all over again.
> 
> OR, is there any standards which I could refer to handle this situation.
> 
> Thanks in advance for your valuable inputs.
> 
> Best Regards,
> U.Nagaraj
> MICROPACK LIMITED,
> Bangalore, INDIA.
> Kindly note: Our domain name has changed to micropack.in from micro- 
> pack.com, please update my email-id in your address book with the new 
> domain name - micropack.in
> 
> [Logo]<http://www.micropack.in>
> 
> __________________________________________________________
> ____________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or 
> [log in to unmask] 
> __________________________________________________________
> ____________
> 
> 
> 
> __________________________________________________________
> ____________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or 
> [log in to unmask] 
> __________________________________________________________
> ____________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2