Hi Chuck,
Thank you for the input. The mask is a LPI, not a dry film, I double
checked the fab notes to be sure. I'll have a chance to look at the next
lot of boards soon as we are expecting the next delivery shortly...
Steve
On Wed, Nov 11, 2015 at 1:17 PM, Chuck Brummer <[log in to unmask]> wrote:
> Steve,
>
> Appears that the lamination of DFSM has forced the SM into the holes. If
> the spray pressure at develop is not adequate it will not clear the mask
> from the barrels.
> Suggest you tell you supplier that this is a problem even if you do not
> reject the parts. They can rework easily if they mask is not cured.
> If I am incorrect, this is screened mask (of your you images looks very
> much like dry film, the other seems a little rough and might be liquid)
> they are spraying mask when the screen "snaps off" and contaminates the pad.
>
> Based on your need you are making a good decision but I would still give
> feedback to the board supplier.
>
>
> Chuck Brummer
> Medical Flex, EMSD
> 8357 Canoga Ave, Canoga Park, CA 91304-2605
> Office: +1 818 734-4930 | Mobile: +1 805 890-8452
> [log in to unmask]
>
>
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
> Sent: Tuesday, November 10, 2015 10:32 AM
> To: [log in to unmask]
> Subject: [EXTERNAL] [TN] Unusual solder mask defect...
>
> Hi All,
>
> We just ran across a soldermask defect that I'm having trouble trying to
> figure out how it may have been caused. We build a .093" thick 8-layer
> assembly for a customer that is pretty picky as far as barrel fill is
> concerned. So we started noticing a problem on one lead of a component that
> we kept seeing no top solder fillet on that usually didn't have a problem.
> Upon further investigation we saw that there was a solder mask ring down
> inside the barrel:
>
> http://stevezeva.homestead.com/Soldermask_plug.jpg
>
> So then I pulled the bare boards that we had in stock and found this:
>
> http://stevezeva.homestead.com/Soldermask_plug_2.jpg
>
> I would say that at least 2/3rds of the boards I looked at had this
> problem. What's kind of weird is that this mask ring would appear at the
> top of the barrel and sometimes at the bottom, but always the same hole.
> The mask is an LPI, and what I'm having a hard time understanding is that
> the mask seems so well imaged around circumference of the pad, how does it
> get cured inside the barrel like that? And why is the ring sometimes at the
> top of the barrel and others down at the bottom?
>
> I was able to clear the plug by carefully using a .033" drill bit under a
> microscope so that I didn't damage anything else in the barrel. I double
> checked the gerbers and there are no inner layer connections, the only
> connection is the trace that you see on the outer layer in the photo.
> Because of time constraints we could not send the boards back to the fab
> vendor (even though I wanted to), but we put the next shipment on hold
> until they inspected for the problem. Why doesn't it surprise me that they
> said that they didn't see the problem? Sheesh...
>
> So I'm just trying to understand what in the process could have caused
> this, a scratch in the artwork maybe?
>
> Steve
>
> --
>
>
> This email and any attachments are only for use by the intended
> recipient(s) and may contain legally privileged, confidential, proprietary
> or otherwise private information. Any unauthorized use, reproduction,
> dissemination, distribution or other disclosure of the contents of this
> e-mail or its attachments is strictly prohibited. If you have received this
> email in error, please notify the sender immediately and delete the
> original.
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
> 3M security scanners have not detected any malicious content in this
> message.
>
> To report this email as SPAM, please forward it to [log in to unmask]
>
--
This email and any attachments are only for use by the intended
recipient(s) and may contain legally privileged, confidential, proprietary
or otherwise private information. Any unauthorized use, reproduction,
dissemination, distribution or other disclosure of the contents of this
e-mail or its attachments is strictly prohibited. If you have received this
email in error, please notify the sender immediately and delete the
original.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|