Hi Dave,
That what exactly my point. It does happen under certain conditions, so I always advise our customers not to start with a very thick layer of intermetallics.
Cheers,
Vladimir
Sent from my BlackBerry 10 smartphone on the Rogers network.
From: David Hillman
Sent: Thursday, September 17, 2015 08:22
To: Vladimir Igoshev
Cc: TechNet E-Mail Forum
Subject: Re: [TN] BGA Reworked Intermetallic
Hi Vlad - the growth rates of IMCs are pretty well known as they follow an Arrhenius equation behavior. The growth of IMCs from 25C -100C is extremely low so unless you have a product service environment that has a high temperature such as 150C for long time periods, you just are not going to "grow" enough IMC thickness to impact solder joint integrity. Having an IMC of 12 microns (400 uinches) is HUGE and clearly not a normal, typical case found in standard electronics production. The biggest issue with having an IMC discussion is that the data doesn't support IMC failure as a typical root cause for solder joints when we start crunching the numbers. I working with one of our industry colleagues and we are pulling together a paper on industry "myths" where we plan on including the topic of IMCs. As you can imagine, its a fun paper to work on and we hope to have it publish in the upcoming year(ish).
Dave
On Wed, Sep 16, 2015 at 9:52 PM, <[log in to unmask]> wrote:
Hi Dave,
As far as I remember I said it's a reverie for disaster. As you know intermetallics will grow over time and a starting point of 10 or so microns doesn't help.
I had several cases of failure (cracked intermetallics) after it grew up to 12-15 microns.
Does it happen all the time? I don't know
May be not, but the cases I had are good enough "argument" , at least for me.
Regards,
Vladimir
Sent from my BlackBerry 10 smartphone on the Rogers network.
From: David Hillman
Sent: Wednesday, September 16, 2015 22:44
To: TechNet E-Mail Forum; Vladimir Igoshev
Subject: Re: [TN] BGA Reworked Intermetallic
Hi Vlad - what data do you have that 10 micron thick layer of IMC results in the failure of the BGA? There is TONS of subjective comments in the published literature but no hard data of failures. As a basic materials engineering principle, IMCs are brittle but that specific material characteristic seems to be the only reason folks make statements that a "thick" IMC is bad. Should we work to keep IMC layers minimized? Absolutely but I don't believe, as technologists, we should keep propagating the myth about thick IMC layers without having published, reviewable data.
Dave Hillman
Rockwell Collins
[log in to unmask]
On Wed, Sep 16, 2015 at 9:38 AM, Vladimir Igoshev <[log in to unmask]> wrote:
10 microns thick layer is a perfect way for a disaster down the road :-).
There are no parameters for E-Ni, but the appearance of the interface and a P-enriched layer is important.
Vladimir
Sent from my BlackBerry 10 smartphone on the Rogers network.
Original Message
From: Victor Hernandez
Sent: Wednesday, September 16, 2015 10:11
To: [log in to unmask]
Reply To: TechNet E-Mail Forum
Subject: Re: [TN] BGA Reworked Intermetallic
On ENIG surface I don't see much of an increase in the IMC formation thickness. However, on Cu it is a different story. I have measured IMC formation greater tham 10 microns. Not sure of the below statement about E-NI parameter. Please explain!!!
Victor,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
Sent: Wednesday, September 16, 2015 8:12 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Reworked Intermetallic
The "magic" Number should stay the same 1-3 micron but you'd also have to keep an eye on what happened to the layer of E-Ni underneath.
Regards,
Vladimir
SENTEC
Sent from my BlackBerry 10 smartphone on the Rogers network.
Original Message
From: Datacom - Juliano Ribeiro
Sent: Wednesday, September 16, 2015 09:09
To: [log in to unmask]
Reply To: TechNet E-Mail Forum
Subject: [TN] BGA Reworked Intermetallic
Hi to all,
When we reworked the BGA, removed the component of the board and replacement another BGA, what's the intermetallic thickness ideal after the rework?
p.s: Our pcb is ENIG finished and the solder is Tin Lead.
_____________________________
Juliano Bettim Ribeiro
DATACOM
ENGENHARIA DE PROCESSOS
Rua América Nº 1000 - Eldorado do Sul - RS CEP: 92990-000
+55 (51) 8446-2135
+55 (51) 3933-3000
Ramal: 3484
[log in to unmask] www.datacom.ind.br
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|