Hi Vlad - the growth rates of IMCs are pretty well known as they follow an
Arrhenius equation behavior. The growth of IMCs from 25C -100C is extremely
low so unless you have a product service environment that has a high
temperature such as 150C for long time periods, you just are not going to
"grow" enough IMC thickness to impact solder joint integrity. Having an IMC
of 12 microns (400 uinches) is HUGE and clearly not a normal, typical case
found in standard electronics production. The biggest issue with having an
IMC discussion is that the data doesn't support IMC failure as a typical
root cause for solder joints when we start crunching the numbers. I
working with one of our industry colleagues and we are pulling together a
paper on industry "myths" where we plan on including the topic of IMCs. As
you can imagine, its a fun paper to work on and we hope to have it publish
in the upcoming year(ish).
Dave
On Wed, Sep 16, 2015 at 9:52 PM, <[log in to unmask]> wrote:
> Hi Dave,
>
> As far as I remember I said it's a reverie for disaster. As you know
> intermetallics will grow over time and a starting point of 10 or so microns
> doesn't help.
>
> I had several cases of failure (cracked intermetallics) after it grew up
> to 12-15 microns.
>
> Does it happen all the time? I don't know
> May be not, but the cases I had are good enough "argument" , at least for
> me.
>
> Regards,
>
> Vladimir
>
> Sent from my BlackBerry 10 smartphone on the Rogers network.
> *From: *David Hillman
> *Sent: *Wednesday, September 16, 2015 22:44
> *To: *TechNet E-Mail Forum; Vladimir Igoshev
> *Subject: *Re: [TN] BGA Reworked Intermetallic
>
> Hi Vlad - what data do you have that 10 micron thick layer of IMC results
> in the failure of the BGA? There is TONS of subjective comments in the
> published literature but no hard data of failures. As a basic materials
> engineering principle, IMCs are brittle but that specific material
> characteristic seems to be the only reason folks make statements that a
> "thick" IMC is bad. Should we work to keep IMC layers minimized? Absolutely
> but I don't believe, as technologists, we should keep propagating the myth
> about thick IMC layers without having published, reviewable data.
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]
>
> On Wed, Sep 16, 2015 at 9:38 AM, Vladimir Igoshev <
> [log in to unmask]> wrote:
>
>> 10 microns thick layer is a perfect way for a disaster down the road :-).
>>
>> There are no parameters for E-Ni, but the appearance of the interface and
>> a P-enriched layer is important.
>>
>> Vladimir
>>
>> Sent from my BlackBerry 10 smartphone on the Rogers network.
>> Original Message
>> From: Victor Hernandez
>> Sent: Wednesday, September 16, 2015 10:11
>> To: [log in to unmask]
>> Reply To: TechNet E-Mail Forum
>> Subject: Re: [TN] BGA Reworked Intermetallic
>>
>> On ENIG surface I don't see much of an increase in the IMC formation
>> thickness. However, on Cu it is a different story. I have measured IMC
>> formation greater tham 10 microns. Not sure of the below statement about
>> E-NI parameter. Please explain!!!
>>
>> Victor,
>>
>> -----Original Message-----
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
>> Sent: Wednesday, September 16, 2015 8:12 AM
>> To: [log in to unmask]
>> Subject: Re: [TN] BGA Reworked Intermetallic
>>
>> The "magic" Number should stay the same 1-3 micron but you'd also have to
>> keep an eye on what happened to the layer of E-Ni underneath.
>>
>> Regards,
>>
>> Vladimir
>>
>> SENTEC
>>
>> Sent from my BlackBerry 10 smartphone on the Rogers network.
>> Original Message
>> From: Datacom - Juliano Ribeiro
>> Sent: Wednesday, September 16, 2015 09:09
>> To: [log in to unmask]
>> Reply To: TechNet E-Mail Forum
>> Subject: [TN] BGA Reworked Intermetallic
>>
>> Hi to all,
>>
>>
>>
>> When we reworked the BGA, removed the component of the board and
>> replacement another BGA, what's the intermetallic thickness ideal after the
>> rework?
>>
>>
>>
>> p.s: Our pcb is ENIG finished and the solder is Tin Lead.
>>
>>
>>
>> _____________________________
>>
>> Juliano Bettim Ribeiro
>>
>> DATACOM
>>
>> ENGENHARIA DE PROCESSOS
>> Rua América Nº 1000 - Eldorado do Sul - RS CEP: 92990-000
>> +55 (51) 8446-2135
>>
>> +55 (51) 3933-3000
>>
>> Ramal: 3484
>> [log in to unmask] www.datacom.ind.br
>>
>>
>>
>>
>> ______________________________________________________________________
>> This email has been scanned by the Symantec Email Security.cloud service.
>> For more information please contact helpdesk at x2960 or [log in to unmask]
>> ______________________________________________________________________
>>
>> ______________________________________________________________________
>> This email has been scanned by the Symantec Email Security.cloud service.
>> For more information please contact helpdesk at x2960 or [log in to unmask]
>> ______________________________________________________________________
>>
>> ______________________________________________________________________
>> This email has been scanned by the Symantec Email Security.cloud service.
>> For more information please contact helpdesk at x2960 or [log in to unmask]
>> ______________________________________________________________________
>>
>> ______________________________________________________________________
>> This email has been scanned by the Symantec Email Security.cloud service.
>> For more information please contact helpdesk at x2960 or [log in to unmask]
>> ______________________________________________________________________
>>
>
>
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|