Hello Everyone,
I have some personal experience working with thiols and they do smell quite pungent in concentrated form. Many are toxic so I would not recommend sniffing concentrated thiols. The odor of these type of compounds ranges from rotten eggs to burnt sulfur. When long chain thiols are applied to metal surfaces, they form a monolayer coating. The thiol group binds to the metal and the chains organize themselves into a monolayer. The concentration of the thiols on the metal surface is relatively low, and the odor disappears. I doubt that even a NIST compliant nose could detect the odor of a thiol monolayer on a metal surface.
Best regards,
Tony Lentz
FCT Assembly
Field Application
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ahne Oosterhof
Sent: Friday, August 14, 2015 10:36 AM
To: [log in to unmask]
Subject: Re: [TN] Solderable Nickel?
There are several kind and sizes, but you should only use one that is NIST compliant.
Ahne.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
Sent: Thursday, August 13, 2015 10:02 AM
To: [log in to unmask]
Subject: Re: [TN] Solderable Nickel?
Drew,
What kind of nose you'd recommend for the " sniff test"? :-)
Vladimir
Sent from my BlackBerry 10 smartphone on the Rogers network.
Original Message
From: Drew meyer
Sent: Thursday, August 13, 2015 12:58
To: [log in to unmask]
Reply To: TechNet E-Mail Forum
Subject: Re: [TN] Solderable Nickel?
Joyce,
I never thought to give the parts the sniff test. There was no noticeable odor in ordinary inspection or solderability testing.
Drew
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: Thursday, August 13, 2015 9:39 AM
To: [log in to unmask]
Subject: Re: [TN] Solderable Nickel?
Some SAM (self assembled molecule) with alkanethiols are known to prevent nickel oxidation... similar to the OSP used for Cu, it might be one of those... just a guess. we are possibly not talking about the nickel we use to get here "solderable"? would be interesting to know the shelf life...i am looking forward for more info. (is it smelly?) jk
> LOL - sometimes our discussions are quite humorous! When we use the
> phrase "nickel is quite solderable if not oxidized" is kinda like
> saying "I can breathe underwater if I am using a scuba tank"! When we
> receive a nickel surface finish on a component it will be oxidized as
> nickel oxide forms very quickly and is very stable. I think the point
> everyone is making is that if you can get the nickel oxide out of the
> way, we have a high probability of making a successful solder joint.
> The real question is what are the component suppliers doing to allow
> use to us to use our standard process flux formulations (aka avoiding
> using aggressive flux
> formulations)
> and not have nickel oxide cause wetting problems? Is there an OSP type
> coating? I did not see any mention of this on the vendor's data sheet.
>
> Dave
>
> On Thu, Aug 13, 2015 at 9:03 AM, Stadem, Richard D. <
> [log in to unmask]> wrote:
>
>> Nickel is quite soluble in solder if not oxidized. There are many
>> methods of preventing oxidation, including immersion gold plating
>> (standard ENIG), OSP, and other organic or polymer coatings that are
>> pre-stripped just prior to processing. This is very common.
>> I am just clarifying this for those who may not understand this
>> thread because your emails seem to indicate that nickel is not
>> solderable, period.
>> While nickel's rate of dissolution into molten solder is much slower
>> than copper, silver, or gold, it is still quite solderable if not
>> oxidized, and must be protected.
>>
>> -----Original Message-----
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
>> Sent: Thursday, August 13, 2015 8:06 AM
>> To: [log in to unmask]
>> Subject: Re: [TN] Solderable Nickel?
>>
>> We are on the same wavelength then:-). In essence, everyone literally
>> solder either to Cu or your Ni.
>>
>> There are only two ways of soldering to Ni I can think of: either
>> have a rather strong flux (as you pointed out), or have something like "OSP"
>> preserving its surface. I've never heard of such thing though but it
>> doesn't mean it can not exist.
>>
>>
>> Regards,
>>
>> Vladimir
>> Sent from my BlackBerry 10 smartphone on the Rogers network.
>> Original Message
>> From: David Hillman
>> Sent: Thursday, August 13, 2015 08:53
>> To: [log in to unmask]
>> Reply To: TechNet E-Mail Forum
>> Subject: Re: [TN] Solderable Nickel?
>>
>> Hi Vlad - let's characterize nickel this way: in general, nickel is
>> solderable with the aggressive fluxes. The majority of the flux
>> formulations used by many of the High Performance OEMs are ROL0
>> materials which traditionally were not very compatible with nickel
>> surface finishes.
>> The flux formulations being used are not aggressive. So I have the
>> some question as Ben - what's different about these new "solderable nickel"
>> surface finishes? I have subjected them to 150C bake for 4 hours and
>> they meet the IPC-JSTD-002 testing criteria. Pretty impressive.
>>
>> Dave
>>
>> On Thu, Aug 13, 2015 at 7:27 AM, Vladimir Igoshev <
>> [log in to unmask]> wrote:
>>
>> > Ni in general is solderable. The clues to on is "for how long"! Are
>> > you sure the parts font have a thin layer of Sn over Ni?
>> >
>> > Regards,
>> >
>> > Vladimit
>> >
>> > Sent from my BlackBerry 10 smartphone on the Rogers network.
>> > Original Message
>> > From: Gumpert, Ben
>> > Sent: Thursday, August 13, 2015 07:35
>> > To: [log in to unmask]
>> > Reply To: TechNet E-Mail Forum
>> > Subject: [TN] Solderable Nickel?
>> >
>> > TechNetters,
>> >
>> > I've received several components recently that were plated with
>> > 'solderable nickel' and to my surprise they soldered just fine
>> > (using a
>> > ROL0 flux).
>> > Anyone know what is going on to keep the nickel from oxidizing?
>> >
>> > Ben
>> >
>> > ___________________________________________________________________
>> > ___ This email has been scanned by the Symantec Email
>> > Security.cloud
>> service.
>> > For more information please contact helpdesk at x2960 or
>> > [log in to unmask]
>> > ___________________________________________________________________
>> > ___
>> >
>> > ___________________________________________________________________
>> > ___ This email has been scanned by the Symantec Email
>> > Security.cloud
>> service.
>> > For more information please contact helpdesk at x2960 or
>> > [log in to unmask]
>> > ___________________________________________________________________
>> > ___
>> >
>>
>> _____________________________________________________________________
>> _ This email has been scanned by the Symantec Email Security.cloud
>> service.
>> For more information please contact helpdesk at x2960 or
>> [log in to unmask]
>> _____________________________________________________________________
>> _
>>
>> _____________________________________________________________________
>> _ This email has been scanned by the Symantec Email Security.cloud
>> service.
>> For more information please contact helpdesk at x2960 or
>> [log in to unmask]
>> _____________________________________________________________________
>> _
>>
>> _____________________________________________________________________
>> _ This email has been scanned by the Symantec Email Security.cloud
>> service.
>> For more information please contact helpdesk at x2960 or
>> [log in to unmask]
>> _____________________________________________________________________
>> _
>>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|