Just you add to what Save said "or to have micro voiding formed at the interface due to either the process of the finish" .
Regards,
Vladimir
Sent from my BlackBerry 10 smartphone on the Rogers network.
Original Message
From: David Hillman
Sent: Tuesday, August 11, 2015 15:50
To: [log in to unmask]
Reply To: TechNet E-Mail Forum
Subject: Re: [TN] immersion silver
Hi Bob - Ag and Sn have a rich intermetallic family so there is very little
risk of having undissolved Ag if the solder volume, reflow time, and reflow
temperature parameters are adequately controlled. The biggest risk of
having an issue with a silver surface finish (or any metallic surface
finish) is have segregation of the surface finish at an interface due to
inadequate soldering process parameters.
Dave
On Tue, Aug 11, 2015 at 8:00 AM, Bob Lazzara <[log in to unmask]>
wrote:
> We've considered...
>
> • the value (if any) of thicker immersion coatings
> • the consequences (if any) of immersion-enriched solder joints.
>
> I'll add that the more immersion coating we accumulate on the PCB at
> fabrication, the more we must fully absorb from the PCB at assembly.
> Failing that invites risk of components joined to some remnant amount of
> immersion coating.
>
> Many may have seen fully wetted component joints that nonetheless pop-off
> revealing residual gold on the PCB terminals. While tin may variably absorb
> into the copper I wonder what would become of undissolved silver (and its
> influence on joint reliability).
>
> Bob Lazzara
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of David Hillman
> Sent: Tuesday, August 11, 2015 8:28 AM
> To: [log in to unmask]
> Subject: Re: [TN] immersion silver
>
> Hi team - well, as usual the truth actually lies in the middle of the
> technical discussion. Supporting Vlad's point, solder is fairly robust to
> silver in terms of degrading integrity influences so in most of our
> soldering situations it's not an issue. Supporting Werner's point, he did
> have a specific case where silver embrittlement of the solder joint was the
> root cause of a series of solder joint failures. Werner and I had long
> discussions on that case as it was very interesting despite being somewhat
> of an odd case. So the final answer is silver can be an issue but it takes
> some specific metallurgical conditions. The immersion silver surface
> finished used today on printed circuit boards will not contribute to the
> degradation of solder joint integrity.
>
> Dave
>
> On Tue, Aug 11, 2015 at 7:02 AM, Vladimir Igoshev <
> [log in to unmask]> wrote:
>
> > Hi Guy,
> >
> > With all due respect to Warner memory, silver IS NOT like gold and
> > DOES NOT cause embrittlement.
> >
> > Therefore, from the reliability point of view it wouldn't matter what
> > thickness of IAg was on a board, as long as we ONLY talking about the
> > amount of Ag which would and up in the joints after re-flow.
> >
> > Regards,
> >
> > Vladimir
> >
> > Sent from my BlackBerry 10 smartphone on the Rogers network.
> > Original Message
> > From: Guy Ramsey
> > Sent: Tuesday, August 11, 2015 07:37
> > To: [log in to unmask]
> > Reply To: [log in to unmask]
> > Subject: Re: [TN] immersion silver
> >
> > If Werner were alive he would be reminding us that silver, like gold,
> > is a contaminate in tin solder.
> > Early finishes, prior to 2005 or so, weren't good for multiple reflows.
> > Some
> > presumed it was too thin.
> > I believe the problem was the durability of the organic additives that
> > retard oxidation of the silver.
> > Not perfect, but it is my preferred surface finish, but not too thick.
> >
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]] On Behalf Of Steven Kelly
> > Sent: Monday, August 10, 2015 3:47 PM
> > To: [log in to unmask]
> > Subject: [TN] immersion silver
> >
> > Hi All,
> > Why would someone choose thick immersion silver over thin? Are these
> > different chemistries? Regards Steve Kelly
> >
> >
> > Phone(O) (416) 750-8433
> > Phone (C) (416) 577-8433
> >
> > If the recipient to whom this e-mail is sent has an NDA with PFC
> > Flexible Circuits Limited this e-mail is considered confidential and
> > is subject to any NDA agreements between the respective parties.
> >
> > See PFC on "How its' Made" in Canada on July 7th at 8 p.m. on the
> > Discovery Channel
> >
> >
> > ______________________________________________________________________
> > This email has been scanned by the Symantec Email Security.cloud service.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
> >
> > ______________________________________________________________________
> > This email has been scanned by the Symantec Email Security.cloud service.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
> > ______________________________________________________________________
> > This email has been scanned by the Symantec Email Security.cloud service.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|