Hi Mumtaz - two things we have seen that are important when soldering
NiPdAu component finishes are (1) soldering temperature/profile. Pd
dissolves much slower into Sn than other elements so running the soldering
temperatures 10 degrees hotter than typical and increasing the soldering
time 3-5 seconds longer than typical can be beneficial; (2) flux
formulation. Some fluxes work better than others when Pd is included in the
soldering situation. Hope this helps.
Dave Hillman
Rockwell Collins
[log in to unmask]
On Thu, Jul 23, 2015 at 10:46 AM, Mumtaz Bora <[log in to unmask]> wrote:
> Dear All, Good Morning, Looking for some knowledge base on soldering
> NiPdAu finished components with low melt solder such as Sn42.0Bi57.6Ag0.4
> to avoid wetting issues on a heavy copper plane board. Any insight and
> advise will be appreciated.
>
> Thank-you
> Mumtaz
> 858-795-0112
> Peregrine Semiconductor
>
>
> CONFIDENTIALITY NOTE: The information transmitted, including attachments,
> is intended only for the person(s) or entity to which it is addressed and
> may contain confidential and/or privileged material. Any review,
> retransmission, dissemination or other use of, or taking of any action in
> reliance upon this information by persons or entities other than the
> intended recipient is prohibited. If you received this in error, please
> contact the sender and destroy any copies of this information.
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|