Hi Chris - great information. One comment, some underfill materials can
actually make things worst so find out if they did any qualification
testing with the underfill material.
Dave
On Thu, Aug 7, 2014 at 1:45 PM, Chris Mahanna <[log in to unmask]> wrote:
> My hypothesis goes something like this
>
> As Dave says "microstructure coarsening is more subdued". I'd add -with
> very little banding compared to the damage accumulated at the Sn grain
> interfaces. That is what I meant about this one being odd. But then
> again... we don't see SnPb failures much these days.
> My suspicion was that (relatively speaking) the sj was born that way - as
> Joyce says: "way off eutectic, yielding high % of high melting phase",
> rather than aged/evolved that way.
>
> I also suspected a relatively static mechanical load caused by residual
> stress in the joints, as the board may not be too stable/flat during
> reflow. Average soldering cool-down rate was probably over 6C/s at the
> time of solidus. These fractures were found in a perimeter column.
>
> This BGA is a small 8M-bit SRAM. I would have thought it to be pretty
> flexible. It is underfilled, which is a wildcard at the moment. We are
> asking for the material part# now.
>
> So the suspicion was on the reballing, but you can see why the confidence
> level is low.
>
> This is actual dirty laundry, so can't say the use environment, but there
> is relatively benign thermal cycling and enough vibe that it should be
> taken into consideration.
>
> Chris
>
>
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of David Hillman
> Sent: Thursday, August 7, 2014 1:10 PM
> To: [log in to unmask]
> Subject: Re: [TN] SJ fracture signature
>
> Yes, Chris, come as clean as you can or we'll send Clump/Kloumpios to
> visit you.
>
> Dave
>
>
> On Thu, Aug 7, 2014 at 11:44 AM, Stadem, Richard D. <
> [log in to unmask]> wrote:
>
> > Okay, Chris. We've done our WAG speculating. Out with your suspicions,
> > we must hear them.
> > dean
> >
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Mahanna
> > Sent: Wednesday, August 06, 2014 1:49 PM
> > To: [log in to unmask]
> > Subject: [TN] SJ fracture signature
> >
> > We see hundreds of cracked solder joints every year, but I can't say
> > that I've ever seen one quite like this. I have some suspicions, but
> > I'll keep them to myself, as to not prejudice the crowd.
> > EDS maps are forthcoming.
> >
> > This is a caught in-the-wild field failure of a 48-pin BGA Reballed to
> > SnPb ENIG on board side Ni barrier on component side
> >
> > http://stevezeva.homestead.com/45268-1.JPG
> >
> > http://stevezeva.homestead.com/45268-2.JPG
> >
> > http://stevezeva.homestead.com/45268-8.JPG
> >
> > Thoughts? And Thanks to Steve!
> >
> >
> > Chris Mahanna
> > President, Technical Manager
> > Robisan Laboratory Inc.
> >
> >
> > ______________________________________________________________________
> > This email has been scanned by the Symantec Email Security.cloud service.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
> > ______________________________________________________________________
> > This email has been scanned by the Symantec Email Security.cloud service.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|