Victor,
Good application of Zyglo for PCBA level analysis. You can try a slight heating
before application to lower the viscosity for better penetration, also try to
pull a vacuum for better coverage. Lastly, the Zyglo contains chlorine
(sometimes excess of 900ppm) and sulfur, so your EDS analysis on the mounts may
show some of these constituents. Lastly, don't forget to send pictures.
Good luck!
Bhanu
On 7/2/2014 8:47 AM, Victor Hernandez wrote:
> Steven,
>
> When conducting a cross section of PTHs and SMT pads I observed pad cratering. It appears that some of the epoxy media was sucked into the pad cratering/fracture/crack but hard to distinguish with a microscope. With the fluorescence Zyglow, ZL-67, dye penetrant, I hope that the dye will be sucked into the carves during the vacuum process, D&P. Since the dye is visible with black light I hope that traces of the Zyglow will shine when the cross section is completed. No harm in trying something NEW!
>
> Victor,
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Steven Creswick
> Sent: Tuesday, July 01, 2014 2:46 PM
> To: [log in to unmask]
> Subject: Re: [TN] Zyglow, ZL-67, dye penetrant
>
> Victor,
>
> I've used the various Zyglo UV dies to check for cracks in ceramic substrates & packages as well as checking for cracks in various Low Temp Co-fired ceramics, but have not had the opportunity to attempt to use it on a PWB laminate.
>
> As 'penetrating' as that stuff is I would almost be surprised if it did not wick down the fibers on a cross-section of a good laminate....
>
> Sometimes a Sharpie magic marker works very well too. Blue is always my favorite. Rinse/wipe with acetone or alcohol, as appropriate
>
> Keep your hands clean!
>
>
> Steve Creswick
> Sr Associate - Balanced Enterprise Solutions http://www.linkedin.com/in/stevencreswick
> 616 834 1883
>
>
>
>
> Original Message
> From: Victor Hernandez
> Sent: Tuesday, July 1, 2014 12:24 PM
> To: [log in to unmask]
> Reply To: TechNet E-Mail Forum
> Subject: [TN] Zyglow, ZL-67, dye penetrant
>
> Fellow TechNetters:
>
> Has anyone use the above stated product in a PWB/PCB cross section to highlight cracks/fractures. Sometimes can be used to substitute Dykeem Steel rule dye.
>
> Victor,
>
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
--
Bhanu Sood
Center for Advanced Life Cycle Engineering (CALCE)
Test Services and Failure Analysis Laboratory
Room 0128, Glenn L. Martin Hall (Building 088)
University of Maryland
College Park, MD 20742
Tel: +1 (301) 405 3498
Fax: +1 (301) 314 9269
e-mail: [log in to unmask]
Skype: calce_umd
website: www.calce.umd.edu/TSFA
Confidentiality Notice: The information contained in this e-mail
and any attachments may be legally privileged and confidential.
If you are not an intended recipient, you are hereby notified that
any dissemination, distribution or copying of this e-mail is strictly
prohibited. If you have received this e-mail in error, please notify
the sender and permanently delete the e-mail and any attachments
immediately. You should not retain, copy or use this e-mail or
any attachment for any purpose, nor disclose all or any part of the
contents to any other person.
---
This email is free from viruses and malware because avast! Antivirus protection is active.
http://www.avast.com
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|