TECHNET Archives

June 2014

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Mon, 2 Jun 2014 21:43:22 +0000
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Zilber Gil <[log in to unmask]>
Message-ID:
Subject:
From:
Zilber Gil <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-8-i"
MIME-Version:
1.0
Parts/Attachments:
text/plain (181 lines)
Soldering other company capacitor on same location has no problem.
I did not try to lowering the temperature. Hand soldering give good results.
Thanks,
Gil


-------- הודעה מקורית --------
מאת: Wayne Thayer
תאריך:02/06/2014 11:52 PM (GMT+02:00)
אל: [log in to unmask]
נושא: Re: [TN] Capacitor - strange soldering behavior

Let's suppose the caps are Pb-free.  And has been pointed out as a
possibility, suppose they heat up faster (or to a higher temperature) than the
pcb.  Is it possible that the alloy created has a higher melting point than
the oven profile is set up for?  If all of that happened, maybe the solder
would cling to the part and refuse to flow back down to the board as the
reflow profile progressed.  In that case, either raising or lowering the
temperature might just fix the issue (as would the previous suggestion by Ioan
of dropping the top-side temperature).  I presume that if you add a little
solder paste and rework these parts that they work fine.  Is that correct?

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Reuven Rokah
Sent: Monday, June 02, 2014 3:30 PM
To: [log in to unmask]
Subject: Re: [TN] Capacitor - strange soldering behavior

Hi Gil,

It seems a component plating failure.
Try to check what is the difference between this capacitor and other one with
good performance.
It seems your problematic cap. have grainy structure plating which that suck
the solder during the solder joint.
Try to work with 220 deg C.


On Mon, Jun 2, 2014 at 6:12 PM, Zilber Gil <[log in to unmask]> wrote:

>  XRF was done on a new part before reflow. Before reflow the surface
> was shine. After reflow it was grayed and porous as seen in the picture.
> Thanks,
>
> Gil
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
> Sent: Monday, June 02, 2014 6:06 PM
> To: [log in to unmask]
> Subject: Re: [TN] Capacitor - strange soldering behavior
>
> Would XRF plating alloy identification work here on a loose part?
>
> Victor,
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of David Hillman
> Sent: Monday, June 02, 2014 9:36 AM
> To: [log in to unmask]
> Subject: Re: [TN] Capacitor - strange soldering behavior
>
> Hi Gil - two questions: (1) Does the capacitor have a barrier layer of
> copper or nickel to prevent the underlying metallization from leaching
> into the solder joint?; (2) Have you completed a cross section to
> assess the solder joint microstructure?
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]
>
>
> On Thu, May 29, 2014 at 9:01 AM, Zilber Gil wrote:
>
> > Hello Technet,
> >
> > While soldering this ceramic capacitor (
> > http://ipc-technet.groupsite.com/gallery/27235), its looks like that
> > the capacitor suck the solder from the PCB`s pad to the capacitor
> > pad and the color is now grayish and porosity. XRF found Sn, Pb, Cu
> > on the capacitor pad. PCB Solderability was good and the profile was
> > SnPb at
> > 225 deg C under Nitrogen. Other capacitors and components on the
> > board look normal with shine soldering.
> > Can anybody seen something like that before? Any ideas?
> >
> > Thanks and have a wonderful weekend.
> >
> > Dr. Gil Zilber
> > Technologist, Elta system Ltd.
> >
> >
> > The information contained in this communication is proprietary to
> > Israel Aerospace Industries Ltd. and/or third parties, may contain
> > confidential or privileged information, and is intended only for the
> > use of the intended addresse thereof. If you are not the intended
> > addressee, please be aware that any use, disclosure, distribution
> > and/or copying of this communication is strictly prohibited. If you
> > receive this communication in error, please notify the sender
> immediately and delete it from your computer.
> >
> > Thank you.
> >
> >
> > ____________________________________________________________________
> > __ This email has been scanned by the Symantec Email Security.cloud
> > service.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ____________________________________________________________________
> > __
> >
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
> The information contained in this communication is proprietary to
> Israel Aerospace Industries Ltd. and/or third parties, may contain
> confidential or privileged information, and is intended only for the
> use of the intended addresse thereof. If you are not the intended
> addressee, please be aware that any use, disclosure, distribution
> and/or copying of this communication is strictly prohibited. If you
> receive this communication in error, please notify the sender immediately
> and delete it from your computer.
>
> Thank you.
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>



--

Best Regards,

*Reuven Rokah*

Mobile: 972-52-6012018
Tel:        972-3-9360688
Fax:          076-5100674
 <http://www.rokah-technologies.com/>[log in to unmask]
[log in to unmask]
www.rokah-technologies.com<http://www.rokah-technologies.com>


This e-mail message is intended for the recipient only and contains
information which is CONFIDENTIAL and which may be proprietary of Rokah
Technologies. If you have received this transmission in error, please inform
me by e-mail, phone or fax, and then please delete all of the original files
and all other copies exist.


______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
The information contained in this communication is proprietary to Israel Aerospace Industries Ltd. and/or third parties, may contain confidential or privileged information, and is intended only for the use of the intended addresse thereof. If you are not the intended addressee, please be aware that any use, disclosure, distribution and/or copying of this communication is strictly prohibited. If you receive this communication in error, please notify the sender immediately and delete it from your computer.

Thank you.


______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2