TECHNET Archives

May 2014

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Graham Naisbitt <[log in to unmask]>
Date:
Tue, 27 May 2014 14:40:39 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
MIME-Version:
1.0
Message-ID:
<C0A99C51937F41FB9BA575626B0B6648@PRECISIOD08B7E>
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; format=flowed; charset="Windows-1252"; reply-type=original
From:
Joe Russeau <[log in to unmask]>
Parts/Attachments:
text/plain (145 lines)
Graham, Graham, Graham,

I about choked on my afternoon tea when I read your post.  I must disagree 
with you that IC is an unsuitable tool.  In fact, I would say it is highly 
suitable for evaluating bare board cleanliness.  And the items you point out 
about bromide and false positives or false negatives are not necessarily a 
function of the tool, but perhaps more from improper use or inexperience 
using the tool or in understanding what it is that is being evaluated.  The 
gist of Rich's question (I think) is regarding what the industry experts 
consider as an appropriate metric for evaluating IC test results.  Rich 
correct me if I am wrong on that.

To add my 2 cents, I have said for many years now that there is no 
one-size-fits-all to this question.  Documents like IPC-5704 provide a 
general guideline for the evaluation of IC data on bare boards, but you have 
to answer the question of how applicable that criteria is for your 
product(s).  If you have no clue of where to begin, then 5704 provides a 
remedial starting point.  As you begin to gather data, take the time to log 
it and evaluate it.  Hopefully, you are pulling data across multiple product 
designs.  I tell clients all the time that every board has its own threshold 
for how much residue it can tolerate.  So if you are only evaluating one 
board type, you can set a misleading standard for your other products.

Case in point, I had a client a couple of years back that had set an IC 
standard so low that none of their products could meet it.  When asked how 
they developed the standard, they told me that their competitor down the 
road used the same standard and they knew if their competitor could meet it, 
so could they.  They neglected to take into account the material and process 
differences they used compared to their competitor AND they never thought to 
factor in their board supplier's process.  They went off assumptions.  We 
still do that in industry even today and make assumptions about what we 
think we know.  In my world, data is king.  So I would suggest that you 
test, re-test and test some more and look across multiple product lines.  I 
would look at different board laminates and different surface finishes and 
would tabulate the data that I collect.  Over time you should begin to see 
what the "typical" cleanliness picture is for your boards and then you will 
have a standard that is relevant to you.  Until then, I would recommend 
consulting the experts and utilize IPC documents as they are suppose to be 
derived from a consensus of industry experts that have knowledge and 
experience in a given area or discipline.

My 2 pennies.

Joe Russeau




----- Original Message ----- 
From: "Graham Naisbitt" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, May 27, 2014 12:11 PM
Subject: Re: [TN] PCB Cleanliness Via Ion Chromatography Poll (informal)


Hi Richard

I was going to respond sooner but, being equally interested in the response, 
thought I would wait to see what was said.

IMHO this is not a suitable test.

My reasoning being that the test is run by washing / “de-ionising” the 
eluent until it squeaks. Then heating it to 80DegC, and immersing the 
specimen / sample into the eluent for 1 hour.

Problem? The laminate closely resembles a sponge, it is hydrophilic and 
contains more ions than you could shake a stick at.

Result? False negatives?

Why? Br could well be leached out through the mask onto the surface….but Br 
is a requirement…

I have had several board fabricators asking for assistance on this matter as 
they are struggling to get anything to pass….. my answer has been: Use SIR 
sir.

It does not discriminate between ionic and non-ionic contamination, it 
simply examines changes to insulation resistance that might be pre-cursors 
of unwanted electro-chemical activity.

Use IC when you need to know what is present that is causing the problem….or 
use FTIR?

Use Process Ionic Contamination Testing (PICT) to control the process. Fast, 
simple, relatively inexpensive and effective.

Always at your service,

BR Graham Naisbitt


On 23 May 2014, at 14:27, Richard Kraszewski <[log in to unmask]> 
wrote:

> I actually sent this out on May  16th, but never got a single response. 
> Hoping that was not due to lack of interest, but rather due to the TechNet 
> being down. Hence, I think I'll try this one more time.
>
> I am  hoping to run an informal " min straw poll " here.
>
> Questions stated  are as follows:
>
>
> 1.       "Is your organization testing  incoming  PCB cleanliness  via 
> ion- chromatography?             Replies such as "YES" or "NO" will 
> suffice, but more detailed explanations are also acceptable.
>
>
>
> 2.       " If testing via IC, do you use IPC -5704 Table 4.1 limits or 
> other?                                                Replies such as " 
> IPC"  or "other"  will suffice, but more detailed explanations are also 
> acceptable.
>
> What's in  it for  you?   I will summarize and post the results after a 
> few days of replies.
>
> Rich  Kraszewski
> Senior Process Engineer
> Plexus
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________ 


---
This email is free from viruses and malware because avast! Antivirus protection is active.
http://www.avast.com


______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2