Parts/Attachments:
text/plain (89 lines)
Hi Phil - ugg, not a fun problem! One suggestion to complete as part of 
the initial homework efforts - using either an XRF system or the SEM, 
confirm that the there is no gold on the pads. Gold diffuses into solder 
at a rate of 100 uinches per second at typical  soldering temperatures. If 
there is no longer gold plating on the pads, that means you did have 
molten solder in contact with the pad at some point of the reflow 
exposure. Your lack of wetted solder could then be a solderability or 
plating issue.  If the gold is still  present on the pad then you could 
have a clogged aperture issue or a component warpage issue (i.e. molten 
solder never came in contact). I always get a bit nervous with the visual 
only inspection assessment as sometimes nickel or tin/nickel IMC can have 
a gold appearance creating confusion.

Dave Hillman 
Rockwell Collins
[log in to unmask]



From:   Phil Bavaro <[log in to unmask]>
To:     <[log in to unmask]>
Date:   03/12/2014 04:22 PM
Subject:        [TN] BGA non wetting pads
Sent by:        TechNet <[log in to unmask]>



Ok, I have a head scratcher.

We have a recently built boards which exhibited 3/4 failing at functional 
test.  The board finish is ENIG, solder mask is SMOBC, material is Hitachi 
(formerly Rogers "Theta"), and we are using a ROHS BGAs reballed with 
Sn63Pb37 spheres and water soluble paste.  Oven profile was 220 C max, 
preheat ramp, etc.

We focused on one BGA which had JTAG capability built into the circuit. 
Comnponent would not respond to JTAG.

The xray inspection did not reveal any distinct anomalies.  Most of my 
group felt the balls had collapsed adequately but I remain the pessimist 
in this situation.  We did not have a board available to have the BGA 
cross sectioned so I was concerned as I thought I say excessive gap 
between the part and the PWB.

We tried reheating one board using the Rework system and bumped up the 
reflow max to 230C.   No help, but the voids in the xrays did grow (as you 
would expect).

Here is where it gets strange....

We remove the part, and seven random BGA's pads are still completely gold 
in color.   Absolutely no solder wetting to these pads.   A few appear to 
have transparent contamination on the pads.  I don't see what I have known 
to be black pad (years ago) and some of these gold pads are bright gold.

I can only think of one scenario and that would be complete misprint on 
seven pads but really doubt that as the cause.

I try to repeat this defect on a solder sample PWB with just paste printed 
and every pad takes solder.

I am trying to send Steve my photos.

Any ideas?

Thanks,

Phil
________________________________
 This message and any attachments are solely for the use of the addressee 
and may contain L-3 proprietary information that may also be defined as 
USG export controlled technical data. If you are not the intended 
recipient, any disclosure, use or distribution of its content is 
prohibited. Please notify the sender by reply e-mail and immediately 
delete this message and any attachments.

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________




______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2