Lloyd,
I will say that I have not seen this kind of phenomena on Parylene coated
products. Parylene has a much lower CTE, it is thinner so there is not a
bulk of material there to act on the part. I think the penetration
depends a great deal on the standoff height. Normal BGAs are no problems.
But as you start getting into finer and finer pitch balls, with lower and
lower sandoff heights, I have seen Parylene coat over a component without
necessarily coating under a component. Especially if you are getting into
flip chips and such.
Doug Pauls
From: "lduso - Diamond-MT.com" <[log in to unmask]>
To: TechNet E-Mail Forum <[log in to unmask]>, Doug Pauls
<[log in to unmask]>
Date: 09/13/2013 10:10 AM
Subject: Re: [TN] Gull wing solder joints and minimum electrical
clearance
Doug
I've never seen any pics with parylene coating, have you? I know I coat
plenty of BGAs with XY. Just curious how well it penetrates.
Lloyd Duso
Diamond-MT
Plant Manager
(814) 535-3505
www.Diamond-mt.com
On Fri, Sep 13, 2013 at 10:59 AM, Douglas Pauls <
[log in to unmask]> wrote:
Yup. That is the picture I show when the design engineer is convinced you
have to coat every ball on a BGA for waterproofness.
Doug Pauls
From: Steve Gregory <[log in to unmask]>
To: <[log in to unmask]>
Date: 09/13/2013 09:14 AM
Subject: Re: [TN] Gull wing solder joints and minimum electrical
clearance
Sent by: TechNet <[log in to unmask]>
Hi Dave!
Hi to you too Doug, got your picture. WOW. I had no idea that happens!
http://stevezeva.homestead.com/SquishedBalls.jpg
So when you coat a board that has BGA's, I take it that just a layer of
coating won't cause this, but if the coating wicks beneath the BGA you
can have problems?
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Friday, September 13, 2013 6:17 AM
To: [log in to unmask]
Subject: Re: [TN] Gull wing solder joints and minimum electrical
clearance
Hi Victor - I don't have an example of what happens to a QFP as Ian
detailed but Doug and I have the same phenomenon for a BGA. Hey Doug
-
can ya send Steve one of the BGA pictures?
Dave Hillman
Rockwell Collins
[log in to unmask]
From: Victor Hernandez <[log in to unmask]>
To: <[log in to unmask]>
Date: 09/13/2013 05:50 AM
Subject: Re: [TN] Gull wing solder joints and minimum electrical
clearance
Sent by: TechNet <[log in to unmask]>
Can you share this phenomenon photo?
Victor,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Fox, Ian
Sent: Friday, September 13, 2013 2:39 AM
To: [log in to unmask]
Subject: Re: [TN] Gull wing solder joints and minimum electrical
clearance
Here's a phenomenon that can occur Richard. On fine pitch QFPs with a
generous volume of solder in the joint or a bulging joint, the presence
of a reasonable thickness of acrylic conformal coating (say 100um)
between the feet of the device, together with regular extended periods
of time below zero degC (say -10 degC) can result in the solder being
extruded out of the joint thus forming a short to the adjacent lead. The
modulus of the acrylic is greater than that of the SnPb at sub zero
temps so the solder is under compression and flows.
Been there and got that particular T-shirt
Regards
Ian
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: 11 September 2013 20:03
To: [log in to unmask]
Subject: Re: [TN] Gull wing solder joints and minimum electrical
clearance
Joyce, how would it affect reliability?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: Wednesday, September 11, 2013 1:18 PM
To: [log in to unmask]
Subject: Re: [TN] Gull wing solder joints and minimum electrical
clearance
More likely effect your reliability than electrical clearance.
Joyce Koo
Researcher
Materials Interconnect Lab
Office: (519) 888-7465 79945
BlackBerry: (226) 220-4760
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Peter Wong
Sent: Wednesday, September 11, 2013 2:06 PM
To: [log in to unmask]
Subject: [TN] Gull wing solder joints and minimum electrical clearance
We have assemblies where gull wing solder joints have so much solder
that along the side joint, the solder connection extends out to the
adjacent leads similar to Figure 5-1, Image C from IPC-A-610E. "the
solder connection to a termination may exhibit a wetting angle exceeding
90 degrees when it is created by the solder contour extending over the
edge of the solderable termination area or solder resist" (We will be
modifying our stencils to reduce the amount printed on these parts in
the future).
There is no IPC-610 spec for this condition so we were thinking that if
the spacing between the solder joints does not violate Minimum
Electrical Clearance, they are acceptable.
Is this a correct acceptability criteria?
Thanks,
Peter
________________________________
The enclosed documents are proprietary items to Silicon Forest
Electronics' (SFE) customers. They shall not be reproduced nor disclosed
for any purpose except as specified in writing from an authorized agent
of SFE. These documents may contain data restricted for export by the
International Traffic in Arms Regulations (ITAR) section of the Arms
Export Control Act (or the Export Administration Act). Violators are
subject to severe criminal penalties.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute
non-public information. Any use of this information by anyone other than
the intended recipient is prohibited. If you have received this
transmission in error, please immediately reply to the sender and delete
this information from your system. Use, dissemination, distribution, or
reproduction of this transmission by unintended recipients is not
authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned.
______________________________________________________________________
Aero Engine Controls is part of the Rolls-Royce Group, whose legal
entity is Rolls-Royce Engine Control Systems Limited which is registered
in England.
Registered office at Moor Lane, PO Box 31, Derby, DE24 8BJ. Company
number 6686268, UK VAT number GB 939 396 075
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|